Bipyridine-derived zwitter-ion multi-site integrated organic silicon, preparation and application and method in catalysis of conversion of low-concentration carbon dioxide

CN118909259AActive Publication Date: 2024-11-08QINGDAO UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411073085.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Existing catalysts exhibit low activity and poor stability in the cycloaddition reaction of low-concentration CO2 with epoxides, and require additional solvents and co-catalysts, making them difficult to apply industrially.

Method used

We developed a bipyridine-derived zwitterionic multisite integrated organosilicon material and prepared the catalyst using a simple and low-cost synthetic method. The catalyst was used to catalyze the synthesis of cyclic carbonates from low-concentration CO2 and epoxides under mild conditions. The catalyst structure includes Lewis basic N to activate CO2, hydrogen bond donors to activate epoxides, and nucleophilic groups to promote ring opening.

Benefits of technology

It achieves highly selective catalytic conversion of low-concentration CO2 into cyclic carbonates under solvent-free and catalyst-free conditions. The catalyst is easy to separate, the raw materials are readily available, the conditions are mild, and it has good potential for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to bipyridine-derived zwitter-ion multi-site integrated organic silicon, preparation and application and method in catalysis of conversion of low-concentration carbon dioxide, and a novel multifunctional organic silicon material rich in Lewis alkaline N, hydrogen bond donors and nucleophilic group multi-element active sites is constructed by designing and regulating the composition of a multi-element precursor. According to the present invention, the carbon dioxide is adopted as the catalyst, and the carbon dioxide and the different substituent epoxides are adopted as the raw materials to synthesize the corresponding cyclic carbonate so as to achieve the high-selectivity catalysis of the cyclic carbonate synthesis under the low-pressure and solvent-free conditions; in addition, the material has the advantages of being easy to separate and recyclable, and the catalytic activity is not obviously reduced after the catalyst is recycled six times. The bipyridine-derived zwitter-ion multi-site integrated organic silicon material disclosed by the invention has excellent dual functions of carbon dioxide adsorption and catalytic conversion, solves the problems of low catalytic activity, poor stability and difficulty in recovery of a current catalyst, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material synthesis catalysis, and specifically relates to a bipyridine-derived zwitterionic multi-site integrated organosilicon and its application and method in preparation and catalysis of low-concentration carbon dioxide conversion. Background Art

[0002] With the continuous acceleration of the industrialization process and the rapid development of the economy, global energy consumption has grown rapidly, which has led to an increase in carbon dioxide (CO2) emissions year by year. It is the main factor causing global warming and seriously threatens the earth's ecosystem and human living environment. Therefore, achieving CO2 emission reduction has become a global challenge facing mankind today. At the same time, CO2, as an abundant, non-toxic and renewable C1 resource, is directly used as a raw material to produce the required chemicals or fuels. It is considered to be a promising method, such as the synthesis of cyclic carbonates by cycloaddition reaction of CO2 and epoxides and the catalytic hydrogenation of CO2 to obtain methanol, ethanol, CO, and CH4, which can improve the current situation of excessive CO2 emissions to a certain extent and realize the resource utilization of CO2. However, the thermodynamic stability and kinetic inertness of CO2 require the participation of efficient catalysts in the reaction. Among them, cyclic carbonates can be used in many fields such as battery electrolytes, green reagents, and industrial plastic synthesis. Therefore, the reaction route of synthesizing cyclic carbonates from CO2 and epoxides has attracted much attention.

[0003] For the synthesis of cyclic carbonates by the cycloaddition reaction of CO2 and epoxides, the route is in line with atom economy and meets the development requirements of green chemistry. Cyclic carbonate products have excellent physical and chemical properties (such as high boiling point, high polarity, low volatility) and good biodegradability, and are widely used in chemical, pharmaceutical and polymer fields. At present, the homogeneous KI catalytic system is widely used in industry, but the production scale of this process is small and the reaction conditions of the catalytic process are harsh (180-200℃, 5-8 MPa). Based on the high thermodynamic stability and kinetic inertness of CO2, the realization of CO2 conversion first requires the design of an efficient catalyst to activate it; in order to realize the cycloaddition reaction under mild conditions and efficiently, the catalyst is also required to have the function of activating epoxides.

[0004] To date, many catalytic systems have been developed for the cycloaddition reaction of CO2 and epoxides. The application of homogeneous catalytic systems is limited by factors such as poor stability and difficulty in separation and recovery. Therefore, heterogeneous catalytic systems with high stability and easy separation are more suitable for industrial applications and have attracted people's attention, such as metal organic frameworks (MOFs), covalent organic frameworks (COFs), periodic mesoporous organosilicon (PMOs) and polyionic liquids (PILs). However, compared with homogeneous catalytic systems, the catalytic activity is lower, and most of them require harsh reaction conditions or the addition of co-catalysts that are difficult to separate and recover to show excellent catalytic activity. In addition, most current studies use high-purity CO2 for reactions, and the purification of CO2 requires complex processes such as absorption, desorption, compression, and transportation, and has high energy consumption and cost. Therefore, the development of new heterogeneous catalysts for direct and efficient conversion of low-concentration CO2 is of great significance for environmental protection.

[0005] Periodic mesoporous organosilicon (PMO) is a highly advanced hybrid porous material with high specific surface area, ordered pore structure and adjustable structure. It has a wide range of applications in heterogeneous catalysis, adsorption, solar cells and drug release. Various group-modified PMO catalysts have also been developed for the cycloaddition reaction of CO2 with epoxides. Voort et al. used a photo-initiated thiol-ene click reaction to click the salen ligand onto the periodic mesoporous organosilicon bridged by thiolethane. The metal-free Salen-PMO showed excellent catalytic performance for the cycloaddition of CO2 to epoxides, but additional dichloromethane solvent and co-catalyst were required during the reaction. Park et al. used N2,N4,N6-tri(3-(triethyloxy)propyl)-1,3,5-triazine-2,4,6-triamine (TBTS) and sodium metasilicate as raw materials, and prepared melamine trisiloxane-bridged periodic mesoporous silicone by cocondensation in the presence of poly(ethylene oxide)-poly(ethylene oxide)-poly(ethylene oxide) triblock copolymer under highly acidic conditions. The organic molecules were integrated into the silica framework to form an organic-inorganic hybrid material, but as a metal-free catalyst, additional solvent still needed to be added to the reaction.

[0006] In summary, providing a periodic mesoporous organosilicon with novel structure, excellent catalytic performance and recyclability, and enabling it to efficiently catalyze low-concentration CO2 to synthesize cyclic carbonates under mild conditions without solvent or catalyst, has great application prospects and challenges. Based on this, we propose this invention. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects existing in the prior art and provide a bipyridine-derived zwitterionic multi-site integrated organosilicon material. A construction method thereof is provided which is simple in synthesis, inexpensive and environmentally friendly, and an application thereof as a catalyst for the cycloaddition reaction of low-concentration carbon dioxide and epoxides and a method for preparing cyclic carbonates by catalyzing the coupling of low-concentration CO2 and epoxides.

[0008] To achieve the above object, the technical solution adopted by the present invention is: Technical Theme 1 A bipyridine-derived zwitterionic multi-site integrated organosilicon material: characterized in that the preparation steps are as follows: S1: Synthesis of 2,2'-bipyridine-5,5'-diamine monomer In this step there are the following sub-steps: Step I: 5-amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid are reacted in toluene, and then post-treated to obtain 1-(2-chloropyridinyl)-5-yl-2,5-dimethyl-1H-pyrrole; Step II: reacting nickel dibromide bis(triphenylphosphine), zinc powder, tetraethylammonium iodide and 1-(2-chloropyridinyl)-5-yl-2,5-dimethyl-1H-pyrrole obtained in step I in tetrahydrofuran solvent, and post-treating to obtain 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine; Sub-step III: reacting the 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine obtained in sub-step II, hydroxylamine hydrochloride, and triethylamine in a mixed solution of ethanol and water, and obtaining a 2,2'-bipyridine-5,5'-diamine monomer through post-treatment; S2: Synthesis of Bipyridine-derived Organosilicon Precursors In tetrahydrofuran, the 2,2'-bipyridine-5,5'-diamine monomer obtained in step III of step S1 is reacted with isocyanatepropyltriethoxysilane in a certain proportion, and after the reaction is completed, the solvent is removed to obtain a bipyridine-based silicon source precursor; S3: Preparation of Bipyridine-Based Periodic Mesoporous Organosilicon The bipyridine-derived organosilicon precursor obtained in step S2 is mixed with tetraethyl silicate, and hydrolyzed and copolymerized in the presence of a surfactant to generate bipyridine-based periodic mesoporous organosilicon; S4: Preparation of zwitterionic bipyridyl-based periodic mesoporous organosilicon The bipyridyl-based periodic mesoporous organosilicon obtained in step S3 is subjected to a nucleophilic addition reaction with a halide by static hydrothermal method to obtain a zwitterionic bipyridyl-based periodic mesoporous organosilicon material, wherein the halide is selected from alkyl halides, brominated C1-C4 alcohols and brominated C1-C4 acids.

[0009] As a further improvement of the present invention, in step S1, sub-step I, the molar ratio of 5-amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid is 1:1-1.4:0.01-0.03; In sub-step II, the molar ratio of nickel dibromide bis(triphenylphosphine), zinc powder, tetraethylammonium iodide and 1-(2-chloropyridinium)-5-yl-2,5-dimethyl-1H-pyrrole is 1:8-8.5:5-5.5:1-1.5; In sub-step III, the molar ratio of 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine to hydroxylamine hydrochloride is 1:25-35; In the step S2, the molar ratio of 2,2'-bipyridine-5,5'-diamine to isocyanatepropyltriethoxysilane is 1:2-2.5; In the step S3, the molar ratio of the bipyridine-derived organosilicon precursor to tetraethyl silicate silicon is 1:15-25; In step S4, the molar ratio of the bipyridyl-based periodic mesoporous organosilicon material to the halide is 1:1-2; and the halide is selected from ethyl bromide, bromoethanol and bromoacetic acid.

[0010] As a further improvement of the present invention, the reaction conditions of 5-amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid in step S1 in step I are 80-120° C. for 2-3 h; In step II, nickel dibromide, zinc powder, tetraethylammonium iodide and 1-(2-chloropyridinium)-5-yl-2,5-dimethyl-1H-pyrrole are reacted at 60-70° C. for 3-5 h; In step III, 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine and hydroxylamine hydrochloride are reacted at 80-120°C for 18-24 h; The reaction conditions of step S2 are: stirring 2,2'-bipyridine-5,5'-diamine monomer and isocyanatepropyltriethoxysilane under a N2 atmosphere at 50-70°C for 2-4 h to form a homogeneous transparent system, and then removing the solvent by rotary evaporation; The reaction conditions of step S3 are: first stirring at 40-50°C for 20-24 h to form a uniform emulsion system; then transferring it to a hydrothermal kettle and statically heating at 100-150°C for 90-100 h; The reaction conditions of step S4 are: adding the halogenated compound dropwise to the toluene solution of the bipyridyl periodic mesoporous organosilicon, stirring at 20-40° C. for 0.5-1 h, then transferring it to a hydrothermal kettle and statically heating it at 100-150° C. for 20-40 h.

[0011] As a further improvement of the present invention, in step S3, the molar ratio of the bipyridine-derived organosilicon precursor to tetraethyl silicate silicon is 1:25; In the step S4, the halogenated compound is selected from bromoethanol.

[0012] As a further improvement of the present invention, the bipyridine-derived zwitterionic multi-site integrated organosilicon material structure is iPMOx-Bpy-R, wherein x is 15, 20, or 25; and R is CH2OH, CH3, or COOH.

[0013] As a further improvement of the present invention, the bipyridine-derived zwitterionic multi-site integrated organosilicon material structure is iPMO 25 -Bpy-CH2OH.

[0014] Technical Theme 2 An application of a bipyridine-derived zwitterionic multi-site integrated organosilicon material as described in Technical Topic 1 in catalyzing low-concentration carbon dioxide and conversion.

[0015] Technical Theme 3 A method for synthesizing cyclic carbonates by catalyzing the reaction of low-concentration carbon dioxide and epoxides using a bipyridine-derived zwitterionic multi-site integrated organosilicon material as described in Technical Topic 1, wherein the bipyridine-derived zwitterionic multi-site integrated organosilicon material is used as a catalyst to synthesize cyclic carbonates by a cycloaddition reaction of epoxides and low-concentration carbon dioxide.

[0016] As a further improvement of the present invention, the structural formula of the epoxide is as follows: , , , , , or .

[0017] As a further improvement of the present invention, the amount of the bipyridine-derived zwitterionic multi-site integrated organosilicon material catalyst is 1 wt%-10 wt% of the mass of the reaction system.

[0018] As a further improvement of the present invention, the cycloaddition reaction temperature is 50-120° C., the reaction pressure is 0.5-3 MPa, and the reaction time is 3-11 h.

[0019] As a further improvement of the present invention, the cycloaddition reaction temperature is 60-120° C., the reaction pressure is 0.5-2.5 Mpa, and the reaction time is 4-9 h.

[0020] As a further improvement of the present invention, the low concentration of carbon dioxide is 10-15%.

[0021] The beneficial effects of adopting the above technical solution are: The unique structure of the catalyst of the present application contains Lewis basic N to activate CO2, hydrogen bond donor (HBD) to activate epoxide and nucleophilic group to promote the ring opening of epoxide, so that the catalytic process can highly selectively catalytically convert low concentration carbon dioxide to synthesize cyclic carbonate under solvent-free and co-catalyst-free conditions. After the reaction is completed, the catalyst and the product can be separated by filtering, thus overcoming the disadvantages of the currently reported catalytic system such as low activity, poor stability, poor cycle performance and dependence on co-catalysts that are difficult to separate. In addition, the raw materials of the present invention are easily available, the conditions are mild, and the synthesis is efficient, so the direct conversion and utilization of industrial low concentration carbon dioxide can be realized, and the catalyst has good potential for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a reaction flow chart of the present invention; Figure 2 The PMO of the present invention 15 -Bpy, PMO 20 -Bpy, PMO 25 -Bpy and iPMO 25 -Bpy-CH2OH infrared spectrum; Figure 3 The PMO of the present invention 15 -Bpy, PMO 20 -Bpy, PMO 25 -Bpy and iPMO 25 -Bpy-CH2OH small angle XRD spectrum; Figure 4 This is a transmission electron microscope image of the porous heterogeneous skeleton material of the present invention, where (ac) is PMO 25 -Bpy transmission electron microscopy image; (d) PMO 25 -Bpy Mapping Overview; the second row (d) has PMO on the right 25 -Mapping diagram of C, N, O, and Si in Bpy; (eg) is iPMO 25 -TEM image of Bpy-CH2OH; the fourth row from left to right are iPMO 25 -Bpy-CH2OH C, N, O, Si, Br mapping diagram, among which PMO 25 -Bpy was prepared in Example 3, iPMO 25 -Bpy-CH2OH was prepared in Example 4. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is clearly and completely described below in conjunction with specific embodiments.

[0024] In this example section, the synthesis route of bipyridine-derived zwitterionic multi-site integrated organosilicon materials is shown in Figure 1 .

[0025] Example 1 Synthesis of 2,2'-bipyridine-5,5'-diamine (Bpy-NH2) monomer 5-Amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid were dissolved in 15 mL of toluene at a molar ratio of 1:1.2:0.01 and stirred for 2.5 h at 110 °C in a Dean-Stark apparatus. After the dark brown reaction mixture was cooled, it was washed with saturated aqueous NaHCO3, water and brine, respectively. After the solution was dried over MgSO4, the solvent was removed in vacuo to give 1-(2-chloropyridinyl)-5-yl-2,5-dimethyl-1H-pyrrole (Intermediate 1).

[0026] Under N2 atmosphere, bis(triphenylphosphine)nickel bromide, zinc powder and tetraethylammonium iodide were suspended in 10 mL THF at a molar ratio of 1:8.5:5 and stirred at room temperature for 30 min. 5 mmol of intermediate 1 dissolved in 10 ml THF at a molar ratio of 1:1 with bis(triphenylphosphine)nickel bromide was slowly added to the mixture using a syringe, and the resulting mixture was stirred at 65°C for 4 h. Then 20 mL of concentrated ammonia, 15 mL of water and 60 mL of dichloromethane were added, and the mixture was stirred for 15 minutes, and the precipitate was filtered to separate the organic layer. The aqueous phase was extracted three times with dichloromethane and combined with the organic phase, and the combined organic phase was washed with water and brine, and the organic phase was dried over MgSO4 to obtain 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine (intermediate 2).

[0027] 1 mmol of intermediate 2, 30 mmol of hydroxylamine hydrochloride, 4 mL of triethylamine, 25 mL of ethanol and 10 mL of water were heated under reflux for 20 h. Then, 30 mmol of hydroxylamine hydrochloride and 2 mL of triethylamine were added, and the solution was further heated under reflux for 24 h. The reaction mixture was cooled to room temperature and then poured into 1N HCl at 0°C to quench. Ethanol was added to the resulting suspension of golden precipitate, the mixture was cooled to 0°C, and stirred at this temperature for 1 h. Thereafter, the golden precipitate was collected, washed with cold ethanol, and dried in vacuo. After drying, the golden precipitate was collected, dissolved in water, adjusted to pH = 12 with 3N sodium hydroxide, and the mixture was extracted with CHCl3, dried over K2CO3, and the solvent was evaporated under reduced pressure to obtain the product as a light yellow solid, i.e., 2,2'-bipyridine-5,5'-diamine, with a yield of 78%.

[0028] Example 2 Synthesis of Bipyridine-derived Organosilicon Precursor (Bpy-Si(OEt)3) 2,2'-Bipyridine-5,5'-diamine was dissolved in 20 mL of anhydrous tetrahydrofuran, and isocyanate propyl triethoxysilane was added under N2 atmosphere, the molar ratio of 2,2'-bipyridine-5,5'-diamine to isocyanate propyl triethoxysilane was 1:2-2.5, and the mixture was stirred at 65°C for 3 h. After the reaction was completed, the tetrahydrofuran solvent was removed by rotary evaporation, and the residue was washed with n-hexane 3 times and dried under vacuum overnight to obtain the bipyridine-derived organosilicon precursor Bpy-Si(OEt)3 with a yield of 93%.

[0029] Example 3 Preparation of Bipyridine-Based Periodic Mesoporous Organosilicon Based on the surfactant template cocondensation method, PMO with different compositions was prepared by adjusting the molar ratio of Bpy-Si(OEt)3 and tetraethyl silicate (TEOS). x -Bpy ( x = 15, 20, 25).

[0030] The template hexadecyltrimethylammonium bromide (CTAB) (5.3 g, 14.4 mmol) was suspended in a solution of 18 ml NH3·H2O and 246 ml deionized water, stirred at 40 ° C for 0.5 h, and a 50 ml ethanol mixture containing 2 mmol Bpy-Si(OEt)3 and 50 mmol TEOS was added dropwise during stirring, and stirred at 40 ° C for 24 h to form a uniform emulsion system. Then it was transferred to a hydrothermal autoclave, statically heated at 120 ° C for 96 h, filtered and separated, and Soxhlet extracted with ethanol hydrochloric acid solution at 60 ° C for 6 h, repeated three times to remove CTAB, and finally PMO was obtained by filtration and vacuum drying. 25 -Bpy, the yield was 88%.

[0031] In this way, by changing the molar ratio of silicon Si (联吡啶衍生基有机硅前驱体) : Si (TEOS) =1:15 and 1:20 prepared PMO 15 -Bpy and PMO 20 -Bpy, with yields of 82% and 85%, respectively.

[0032] Example 4 Preparation of zwitterionic bipyridyl-based periodic mesoporous organosilicon 0.05 g PMOx-Bpy was dispersed in 10 mL toluene, 4 mmol 2-bromoethanol was added dropwise, stirred at room temperature for 30 min, transferred to an autoclave, statically heat treated at 120 °C for 24 h, filtered and separated, washed with deionized water and methanol to remove unreacted products. After vacuum drying at 60 °C for 5 h, a yellow-brown solid was collected and labeled as iPMOx-Bpy-R (x = 15, 20, 25; R = CH2OH). Catalyst iPMO 15 -Bpy-CH2OH, iPMO 20 -Bpy-CH2OH, iPMO 25 -Bpy-CH2OH yields were 80%, 82%, and 89%, respectively. X -Bpy-COOH (x = 15, 20, 25) and iPMO X -Bpy-CH3 (x = 15, 20, 25) are respectively composed of PMO X -Bpy (x = 15, 20, 25) is prepared by reaction with bromoacetic acid and ethyl bromide, catalyst iPMO 20 -Bpy-COOH and iPMO 15 -Bpy-CH3, with yields of 85% and 79%, respectively.

[0033] Example 5 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH2OH0.0174 g, accounting for 6 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 1.0 MPa, the reactor oil bath was heated to 70°C, and the reaction was continued for 8 hours; after the reaction, the reactor was cooled to room temperature in an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 85%, and the selectivity was ≥99%.

[0034] Example 6 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25-Bpy-CH2OH0.0232 g, accounting for 8 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 2.0 MPa, the reactor oil bath was heated to 100 °C, and the reaction was continued for 4 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 88%, and the selectivity was ≥99%.

[0035] Example 7 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH2OH0.0174 g, accounting for 6 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 1.0 MPa, the reactor oil bath was heated to 110 ℃, and the reaction was continued for 6 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 94%, and the selectivity was ≥99%.

[0036] Example 8 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH2OH0.0116 g, accounting for 4 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to remove the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 2.0 MPa, the reactor oil bath was heated to 100 °C, and the reaction was continued for 6 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 98%, and the selectivity was ≥99%.

[0037] Example 9 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25-Bpy-CH2OH0.0232 g, accounting for 8 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 0.5 MPa, the reactor oil bath was heated to 80°C, and the reaction was continued for 7 hours; after the reaction, the reactor was cooled to room temperature in an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 82%, and the selectivity was ≥99%.

[0038] Example 10 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH2OH0.0290 g, accounting for 10 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 1.5 MPa, the reactor oil bath was heated to 120 ℃, and the reaction was continued for 4 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 88%, and the selectivity was ≥99%.

[0039] Embodiment 11 Take the reactant propylene oxide and the catalyst iPMO prepared by the method described in Example 4 15 -Bpy-CH3 was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH30.0116 g, accounting for 4 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to remove the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 1.0 MPa, the reactor oil bath was heated to 90 °C, and the reaction was continued for 7 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 83%, and the selectivity was ≥99%.

[0040] Example 12 Take the reactant propylene oxide and the catalyst iPMO prepared by the method described in Example 4 20 -Bpy-COOH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25-Bpy-COOH 0.0116 g, accounting for 4 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; thereafter, 10% CO2 gas was introduced to maintain a constant pressure of 1.0 MPa, the reactor oil bath was heated to 90 °C, and the reaction was continued for 7 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 86%, and the selectivity was ≥99%.

[0041] Embodiment 13 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH2OH0.0116 g, accounting for 4 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to expel the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 2.5 MPa, the reactor oil bath was heated to 70 ℃, and the reaction was continued for 9 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 89%, and the selectivity was ≥99%.

[0042] Embodiment 14 Take the reactant propylene oxide and the catalyst iPMO prepared in Example 4 25 -Bpy-CH2OH was added into a 25 mL stainless steel autoclave lined with polytetrafluoroethylene, including 5.0 mmol (0.29 g) of propylene oxide, 5.0 mmol (0.29 g) of iPMO 25 -Bpy-CH2OH0.0116 g, accounting for 4 wt% of the reactant mass; 10% CO2 gas was slowly introduced into the reactor to remove the residual air inside; then, 10% CO2 gas was introduced to keep the pressure constant at 1.0 MPa, the reactor oil bath was heated to 90 ℃, and the reaction was continued for 7 hours; after the reaction was completed, the reactor was cooled to room temperature with an ice water bath, and the product was quantitatively analyzed by gas chromatography-mass spectrometry, the yield of propylene carbonate was 96%, and the selectivity was ≥99%.

[0043] Embodiment 15 The experimental process was the same as in Example 14, using the iPMO prepared in Example 4 25 -Bpy-CH2OH was used as the catalyst. Under the conditions of 90 ℃, 1.0 MPa, 5.0 mmol of epoxide and 4 wt% of catalyst, different epoxides were selected to react with carbon dioxide. The results are shown in Table 1.

[0044] Table 1 iPMO 25 -Bpy-CH2OH catalyzed cycloaddition reaction of carbon dioxide with different epoxides Examples 16-21 The specific experimental conditions and steps were the same as those in Example 14, except that the catalyst iPMO 25 -Bpy-CH2OH was replaced by iPMO recovered in Example 14 25 -Bpy-CH2OH, 6 cycles were performed under the same conditions, and the results are shown in Table 2.

[0045] Table 2 Experimental results of catalyst recycling in Examples 16-21 Embodiment 22 Table 3 below compares one of the bipyridine-derived zwitterionic multi-site integrated organosilicon proposed in the present invention with other porous organic polymers reported in the literature. The catalyst type was replaced by the catalytic method in Example 14, and the yield and selectivity were measured as follows: Table 3 Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A bipyridine-derived zwitterionic multi-site integrated organosilicon material, characterized in that The preparation steps are as follows: S1: Synthesis of 2,2'-bipyridine-5,5'-diamine monomer In this step there are the following sub-steps: Step I: 5-amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid are reacted in toluene, and then post-treated to obtain 1-(2-chloropyridinyl)-5-yl-2,5-dimethyl-1H-pyrrole; Step II: reacting nickel dibromide bis(triphenylphosphine), zinc powder, tetraethylammonium iodide and 1-(2-chloropyridinyl)-5-yl-2,5-dimethyl-1H-pyrrole obtained in step I in tetrahydrofuran solvent, and post-treating to obtain 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine; Sub-step III: reacting the 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine obtained in sub-step II, hydroxylamine hydrochloride, and triethylamine in a mixed solution of ethanol and water, and post-treating to obtain a 2,2'-bipyridine-5,5'-diamine monomer; S2: Synthesis of Bipyridine-derived Organosilicon Precursors In tetrahydrofuran, the 2,2'-bipyridine-5,5'-diamine monomer obtained in step III of step S1 is reacted with isocyanatepropyltriethoxysilane in a certain proportion, and after the reaction is completed, the solvent is removed to obtain a bipyridine-based silicon source precursor; S3: Preparation of bipyridine-based periodic mesoporous organosilicon The bipyridine-derived organosilicon precursor obtained in step S2 is mixed with tetraethyl silicate, and hydrolyzed and copolymerized in the presence of a surfactant to generate bipyridine-based periodic mesoporous organosilicon; S4: Preparation of zwitterionic bipyridyl-based periodic mesoporous organosilicon The bipyridyl-based periodic mesoporous organosilicon obtained in step S3 is subjected to a nucleophilic addition reaction with a halide by static hydrothermal method to obtain a zwitterionic bipyridyl-based periodic mesoporous organosilicon material, wherein the halide is selected from alkyl halides, brominated C1-C4 alcohols and brominated C1-C4 acids.

2. The bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 1, characterized in that: In step S1, sub-step I, the molar ratio of 5-amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid is 1:1-1.4:0.01-0.03; In sub-step II, the molar ratio of nickel dibromide bis(triphenylphosphine), zinc powder, tetraethylammonium iodide and 1-(2-chloropyridinium)-5-yl-2,5-dimethyl-1H-pyrrole is 1:8-8.5:5-5.5:1-1.5; In sub-step III, the molar ratio of 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine to hydroxylamine hydrochloride is 1:25-35; In the step S2, the molar ratio of 2,2'-bipyridine-5,5'-diamine to isocyanatepropyltriethoxysilane is 1:2-2.5; In the step S3, the molar ratio of the bipyridine-derived organosilicon precursor to tetraethyl silicate silicon is 1:15-25; In step S4, the molar ratio of the bipyridyl-based periodic mesoporous organosilicon material to the halide is 1:1-2; and the halide is selected from ethyl bromide, bromoethanol and bromoacetic acid.

3. The bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 1, characterized in that : In step S1, the reaction conditions of 5-amino-2-chloropyridine, 2,5-hexanedione and p-toluenesulfonic acid in step I are 80-120° C. for 2-3 h; In step II, nickel dibromide, zinc powder, tetraethylammonium iodide and 1-(2-chloropyridinium)-5-yl-2,5-dimethyl-1H-pyrrole are reacted at 60-70° C. for 3-5 h; In step III, 5,5'-bis(2,5-dimethyl-1H-pyrrole)-2,2'-bipyridine and hydroxylamine hydrochloride are reacted at 80-120°C for 18-24 h; The reaction conditions of step S2 are: stirring 2,2'-bipyridine-5,5'-diamine monomer and isocyanatepropyltriethoxysilane under a N2 atmosphere at 50-70°C for 2-4 h to form a homogeneous transparent system, and then removing the solvent by rotary evaporation; The reaction conditions of step S3 are: first stirring at 40-50°C for 20-24h to form a uniform emulsion system; then transferring it to a hydrothermal kettle and statically heating at 100-150°C for 90-100h; The reaction conditions of step S4 are: adding the halogenated compound dropwise to the toluene solution of the bipyridyl periodic mesoporous organosilicon, stirring at 20-40° C. for 0.5-1 h, then transferring it to a hydrothermal kettle and statically heating it at 100-150° C. for 20-40 h.

4. The bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 1, characterized in that: In the step S3, the molar ratio of the bipyridine-derived organosilicon precursor to tetraethyl silicate silicon is 1:25; In the step S4, the halogenated compound is selected from bromoethanol.

5. Use of the bipyridine-derived zwitterionic multi-site integrated organosilicon material as claimed in any one of claims 1 to 4 in catalyzing the conversion of low-concentration carbon dioxide.

6. A method for synthesizing cyclic carbonates by catalyzing the reaction of low-concentration carbon dioxide and epoxides using the bipyridine-derived zwitterionic multi-site integrated organosilicon material as described in any one of claims 1 to 4, characterized in that Cyclic carbonates were synthesized by cycloaddition reaction of epoxides and low-concentration carbon dioxide using bipyridine-derived zwitterionic multi-site integrated organosilicon materials as catalysts.

7. The method for synthesizing cyclic carbonate by reacting low-concentration carbon dioxide with epoxide catalyzed by bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 6, characterized in that: The structural formula of the epoxide is as follows: , , , , , or .

8. The method for synthesizing cyclic carbonate by reacting low-concentration carbon dioxide with epoxide catalyzed by bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 6, characterized in that: The bipyridine-derived zwitterionic multi-site integrated organosilicon material catalyst is used in an amount of 1 wt % to 10 wt % of the mass of the reaction system.

9. The method for synthesizing cyclic carbonate by reacting low-concentration carbon dioxide with epoxide catalyzed by bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 6, characterized in that The cycloaddition reaction temperature is 60-120° C., the reaction pressure is 0.5-2.5 Mpa, and the reaction time is 4-9 h.

10. The method for synthesizing cyclic carbonate by reacting low-concentration carbon dioxide with epoxide catalyzed by bipyridine-derived zwitterionic multi-site integrated organosilicon material according to claim 6, characterized in that: The low concentration of carbon dioxide is 10-15%.

Citation Information

Patent Citations

  • Method for predicting performance of metal organic framework material for catalyzing carbon dioxide

    CN113689918A

  • Cyclotriphosphazene derivative silicon-based solid amine material and application of cyclotriphosphazene derivative silicon-based solid amine material in catalyzing coupling of carbon dioxide and epoxide to prepare cyclic carbonate

    CN117258841A

  • Method for reducing carbon dioxide, photocatalyst for reduction, and method for producing photocatalyst for reduction

    JP2013180943A