SiCN precursor, deformation-controlled ceramic-based composite material and preparation method

By preparing SiCN precursor under solvent-free conditions and compounding it with two-dimensional carbon cloth, using volatile components and active fillers to control deformation, the deformation and crack problems of ceramic matrix composite materials during the pyrolysis process is solved, and high ceramic production is achieved Preparation of SiCN-based ceramic composite materials with low cost.

CN118909261AInactive Publication Date: 2024-11-08HUNAN TIANYA TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411140006.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118909261A_ABST
    Figure CN118909261A_ABST
Patent Text Reader

Abstract

The invention provides a SiCN precursor, a deformation-controlled ceramic-based composite material and a preparation method. Comprising the following steps: preparing a SiCN ceramic precursor; adding a volatile component, an active filler and a peroxide cross-linking agent into the SiCN precursors with different compositions to form a mixed system; the prepared precursor mixed system and carbon cloth are subjected to hot-pressing cross-linking curing molding through a film coating method; cracking the formed composite material fixed by the tool in a cracking atmosphere; the composite material is subjected to densification treatment by dipping a low-viscosity SiCN precursor and then cracking. The ceramic conversion rate is ensured, and meanwhile, the occurrence of pores, cracks and deformation in a material matrix is reduced. By adding volatile components, a gas overflow channel is formed in a matrix, thermal stress is released, pores, cracks and deformation in the material are reduced, the binding force between the ceramic matrix and carbon fibers can be enhanced through formation of cracked carbon in the ceramization process, and meanwhile, matrix shrinkage caused by component volatilization can be made up through added active filler; further, the preparation of the deformation-controlled ceramic-based composite material is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of ceramic-based composite material preparation, and relates to a SiCN precursor, a controlled deformation ceramic-based composite material, and a preparation method. Background Art

[0002] With the continuous innovation and progress of science and technology, the aerospace industry has also developed rapidly. A variety of new functional or structural materials have begun to enter this field, and this field has also put forward new requirements for materials. Ceramic-based composites are a type of functional structural materials that use ceramics as a matrix and composite various fibers. Advanced ceramics have excellent properties such as high temperature resistance, high strength and hardness, relatively light weight, and corrosion resistance. Composites with high-strength and high-elasticity fibers can further improve the toughness and reliability of ceramics. Compared with traditional thermal structural materials (such as metal materials and alloy materials), ceramic-based composites show higher temperature resistance and oxidation resistance, and therefore have become the first choice for thermal structural materials.

[0003] Carbon fiber reinforced ceramic matrix composites use carbon fiber as reinforcement, and have the excellent properties of carbon fiber and ceramic matrix, showing excellent properties such as high strength, high toughness, high temperature resistance, thermal shock resistance, light weight and oxidation resistance. It is also one of the most representative high-temperature thermal structural composite materials. Traditional powder sintering and hot pressing sintering are currently the more commonly used methods for preparing ceramic matrix composites, but their sintering temperature is high and it is inevitable to damage the carbon fiber during the preparation process, which in turn affects the performance of the final product. Ceramic precursors are not only highly controllable in molecular structure and chemical composition, but can also be processed by traditional polymer molding technology. In addition, ceramic precursors have good combination with reinforcement and low ceramicization temperature, which is not easy to damage the fiber. Therefore, ceramic precursors have received widespread attention in the preparation of ceramic matrix composites. Polymer-converted SiCN ceramics show good high-temperature stability, oxidation resistance, creep resistance and excellent mechanical properties. At the same time, they have good high-temperature semiconductor properties, excellent piezoresistive effect and other characteristics. Therefore, carbon fiber reinforced ceramic matrix composites prepared with SiCN as the matrix have also become one of the important solutions for thermal structural composite materials. Polymer Infiltration Pyrolysis (PIP) is an important process for preparing composite materials by impregnating carbon fiber fabrics in polymer precursor solution, curing and pyrolysis, which can realize the preparation of large-scale and complex-shaped ceramic materials. The performance of ceramic precursors will directly affect the performance and application of the final product, so the regulation of precursor performance is also an important topic in ceramic-based composites.

[0004] Although the precursors have many advantages in the preparation of ceramic matrix composites, the organic components in the precursors will escape quickly during the pyrolysis process, which is often accompanied by sample deformation, shrinkage and cracks. The surface morphology and accuracy of the sample are also closely related to the escape of organic components and the release of thermal stress in the system. Therefore, controlling the deformation, shrinkage and cracks of the sample while ensuring the ceramic conversion rate is also a practical problem that needs to be solved urgently. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a SiCN precursor and a ceramic-based composite material with controlled deformation, wherein the SiCN precursor is prepared under solvent-free conditions using cheap raw materials and simple processes, and the SiCN precursor for coating and impregnation is prepared by adjusting the monomer ratio; a volatile component (a low melting point substance or an organic solvent), an active filler and a peroxide cross-linking agent are added to SiCN precursors of different compositions, and then the precursors are composited with a two-dimensional carbon cloth by a coating method, and after being cracked under a certain system, the precursors are densified by multiple PIP processes, so as to prepare a SiCN-based ceramic composite material with low cost, low deformation and low porosity and high ceramic yield.

[0006] To achieve the above objectives, the present application provides a SiCN precursor, a controlled deformation ceramic matrix composite material and a preparation method, wherein: A method for preparing a SiCN precursor comprises the following steps: 1) Add dichlorosilane, trichlorosilane and hexamethyldisilazane into a dry reaction container filled with inert gas, and stir at room temperature for 30 minutes to fully mix the components; wherein the molar ratio of dichlorosilane to trichlorosilane is (1:0)-(1:1), and the molar ratio of the sum of silicon-chlorine bonds in dichlorosilane and trichlorosilane to the silicon-nitrogen bonds in hexamethyldisilazane is (1:1)-(1:2); 2) Heat the reaction system in an oil bath to a slightly boiling state and reflux for 2-6 hours; 3) The unreacted monomers, salts generated during the reaction and precursor oligomers are removed from the above reaction solution by vacuum distillation to obtain a SiCN precursor with side active groups and controllable branching degree.

[0007] In one possible implementation manner, in the method for preparing a SiCN precursor provided in an embodiment of the present application, the dichlorosilane is a mixture of one or more of methyl hydrogen dichlorosilane, methyl vinyl dichlorosilane, methyl phenyl dichlorosilane and diphenyl dichlorosilane.

[0008] A SiCN precursor is prepared by the above-mentioned method for preparing the SiCN precursor.

[0009] A method for preparing a deformation-controlled ceramic-based composite material comprises the following steps: 1) Chemical vapor deposition method was used, with methane as the gas source, at a temperature of 1000 o C, depositing cracked carbon on the surface of the two-dimensional carbon cloth for 2-6 hours to form a two-dimensional carbon fiber preform containing a cracked carbon layer; 2) dissolving the high-viscosity SiCN precursor prepared by the above method, the peroxide initiator and the volatile components in an organic solvent, and then uniformly dispersing the active filler in the above solution system; 3) Remove the organic solvent introduced in step 2) by vacuum rotary evaporation, the vacuum degree is 10-120Pa, and the temperature is lower than the boiling point of the organic solvent by ~10 o C; 4) The precursor mixture system from which the organic solvent is removed in step 3) is layered with the two-dimensional carbon fiber preform prepared in step 1) by a coating method, and then hot-pressed and cross-linked to cure at a curing temperature of 150-300 o C, curing pressure is 0.1-2MPa, and holding time is 4-8h; 5) Fix the composite material cured in step 4) with a tool and pyrolyze it in a pyrolysis atmosphere at a pyrolysis temperature of 900-1400 o C, the holding time is 2-4h, and a SiCN ceramic-based composite material with pores is obtained; 6) A low-viscosity liquid SiCN precursor prepared by the above method is used as an impregnating agent. The porous SiCN ceramic-based composite material obtained in step 5) is impregnated at room temperature for 2-4 hours under 0.1 MPa and then cracked. The impregnation and cracking cycles are 4-10 rounds to densify the ceramic-based composite material.

[0010] In one possible implementation manner, in the method for preparing a ceramic-based composite material with controlled deformation provided in an embodiment of the present application, in step 1): The two-dimensional carbon cloth is woven from at least one of T300-grade carbon fiber, T700-grade carbon fiber, T800-grade carbon fiber, T1000-grade carbon fiber and M40J-grade carbon fiber.

[0011] In one possible implementation manner, in the method for preparing a ceramic-based composite material with controlled deformation provided in an embodiment of the present application, in step 2): The peroxide initiator is a mixture of one or more of diisopropylbenzene peroxide, benzoyl peroxide, di-tert-butyl peroxide and diisopropylbenzene hydroperoxide.

[0012] In one possible implementation manner, in the method for preparing a ceramic-based composite material with controlled deformation provided in an embodiment of the present application, in step 2): The volatile component is one or more of furan, low molecular weight polycarbosilane or low molecular weight polysilazane, and the added amount is 1-8wt.% of the mass of the SiCN precursor.

[0013] In one possible implementation manner, in the method for preparing a ceramic-based composite material with controlled deformation provided in an embodiment of the present application, in step 2): The active filler is a mixture of one or more of B, Si, Al, Ti, Mo, CrSi2, MoSi2, AlN, and B4C, and the amount of the active filler added is 1%-10wt.% of the content of the SiCN precursor.

[0014] In one possible implementation manner, in the method for preparing a ceramic-based composite material with controlled deformation provided in an embodiment of the present application, in step 5), the cracking atmosphere is one of nitrogen, ammonia and argon.

[0015] A controlled deformation ceramic matrix composite material is prepared by the above-mentioned controlled deformation ceramic matrix composite material preparation method.

[0016] Beneficial effects of this application: 1. A SiCN precursor with controllable side-active groups and branching degree was prepared by adjusting the ratio of chlorosilane monomers, and small molecules and oligomers were removed by vacuum distillation. Active fillers and volatile components were added at the same time to achieve a high ceramic yield while reducing the deformation, shrinkage and cracking of ceramic-based composite materials. Compared with the ~50% ceramic conversion rate of most precursors, the ceramic conversion rate of the precursor composite system can reach more than 70% due to the synergistic effect of the adjustable side-active groups and branching degree, the addition of active fillers and the removal of small molecules and oligomers. The high ceramic yield makes it possible to achieve the densification of the composite material through a low number of PIP processes, thereby improving the densification efficiency of the composite material and shortening the preparation time.

[0017] 2. The introduction of volatile components into the precursor can effectively reduce the occurrence of deformation, shrinkage and cracks. The slow pyrolysis or volatilization process of organic components or low-boiling point components at lower temperatures can produce fine pores, which is conducive to the release of thermal stress. In addition, since the escape of components can provide a channel for the escape of organic gases in the precursor at high temperatures, it helps to reduce large deformation and cracking, and improve the surface morphology and dimensional accuracy of the final pyrolysis sample. The addition of active fillers can not only make up for the mass loss caused by volatile components, but also fill the pores formed during the pyrolysis of the precursor. Therefore, it is possible to achieve a high ceramic yield while reducing the occurrence of system deformation, shrinkage and cracks.

[0018] 3. The coating and impregnating agent used in the preparation of SiCN ceramic-based composite materials are both homemade SiCN precursors, but the composition ratio of the two is different. The price of monomers and cross-linking agents is relatively low, and the development cost of other precursors represented by SiCN precursors is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art description are briefly introduced below. The drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor.

[0020] Figure 1 Thermogravimetric curve of Example 1; Figure 2 The thermogravimetric curve of Example 2; Figure 3 The thermogravimetric curve of Example 3; Figure 4 The NMR of Example 2 1 H spectrum. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the present application clearer, the technical solutions in the embodiments of the present application will be described in more detail below in conjunction with the drawings in the preferred embodiments of the present application. In the drawings, the same or similar reference numerals throughout represent the same or similar parts or parts with the same or similar functions. The described embodiments are part of the embodiments of the present application, not all of the embodiments. The embodiments described below with reference to the drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limitations on the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0022] The purpose of the present invention is to provide a method for preparing a SiCN precursor and a ceramic-based composite material with controlled deformation. The SiCN precursor is prepared under solvent-free conditions using cheap raw materials and simple processes, and the SiCN precursor for coating and impregnation is prepared by adjusting the monomer ratio; volatile components (low melting point substances or organic solvents), active fillers and peroxide cross-linking agents are added to SiCN precursors of different compositions and then composited with two-dimensional carbon cloth, which is densified by multiple PIP processes after being cracked under a certain system to prepare a SiCN-based ceramic composite material with low cost, low deformation and low porosity and high ceramic yield.

[0023] To achieve the above object, the present invention provides a method for preparing a SiCN precursor and a SiCN ceramic-based composite material with controlled deformation, and the technical scheme is as follows: Studies have shown that the side chain composition and branching degree of ceramic precursors will affect the ceramic yield of the precursor, the composition, structure and properties of the ceramic material. When the side groups contain active groups such as Si-H and Si-CH=CH2, the precursor has a higher ceramic yield. At the same time, an increase in branching degree also helps to improve the ceramic yield of the precursor.

[0024] Based on this, the present invention provides a method for preparing a precursor with controllable side-active groups and branching degree and a method for preparing a SiCN ceramic-based composite material with controlled deformation. In the first aspect, polysilazane is prepared by aminolysis: The chlorosilane monomers include dichlorosilane and methyltrichlorosilane, and the nitrogen source is hexamethyldisilazane, wherein the molar ratio of dichlorosilane to trichlorosilane is (1:0)-(1:1), and the molar ratio of the silicon-chlorine bonds in dichlorosilane and trichlorosilane to the silicon-nitrogen bonds in hexamethyldisilazane is (1:1)-(1:2), preferably 1:1.5.

[0025] The dichlorosilane includes one or more of methylhydrogendichlorosilane, methylvinyldichlorosilane, methylphenyldichlorosilane and diphenyldichlorosilane.

[0026] The preparation steps of SiCN precursor are as follows: 1) Add different proportions of dichlorosilane, trichlorosilane and hexamethyldisilazane in a dry reaction container filled with inert gas, and stir at room temperature for 30 min to fully mix the components; 2) Heating in an oil bath to bring the reaction system to a slightly boiling state, reflux for 2-6 h, preferably 2 h; 3) The unreacted monomers, salts generated during the reaction and precursor oligomers are removed from the above reaction solution by vacuum distillation to obtain a SiCN precursor with side active groups and controllable branching degree.

[0027] 4) By adjusting the feed ratio of dichlorosilane and trichlorosilane, SiCN precursors with different side groups and branching degrees can be obtained to meet the requirements of coatings and PIP impregnants for preparing composite materials. In a second aspect, a ceramic matrix composite material with controlled deformation is prepared based on the SiCN precursor prepared above, comprising the following steps: 1) A layer of pyrolytic carbon is deposited on the surface of the two-dimensional carbon cloth by chemical vapor deposition (the pyrolytic carbon deposition layer uses methane as the gas source, 1000 oC deposits cracked carbon on the surface of the carbon cloth for 2-6 h), forming a carbon fiber fabric containing a cracked carbon layer (the carbon cloth is woven from at least one carbon fiber of grade T300, grade T700, grade T800, grade T1000 or grade M40J); 2) dissolving a high viscosity (viscosity higher than 100000 mPa·s) SiCN precursor, a peroxide initiator (at least one of diisopropylbenzene peroxide, benzoyl peroxide, di-tert-butyl peroxide, and diisopropylbenzene hydroperoxide) and a volatile component (one or more of furan, low molecular weight polycarbosilane or low molecular weight polysilazane, added in an amount of 1-8 wt.% of the precursor mass) in an organic solvent (one of alkanes or toluene), and then uniformly dispersing an active filler (one or more of single substance B, Si, Al, Ti, Mo, intermetallic compounds such as CrSi2, MoSi2 and ceramic composites such as AlN, B4C, etc., the amount of the active filler added is 1%-10 wt% of the precursor content) in the above solution system; 3) Vacuum evaporation to remove the organic solvent introduced in step 2 (vacuum degree 10-120 Pa, temperature below the boiling point of the organic solvent ~10 o C); 4) The precursor mixed system from which the organic solvent is removed in step 3 is pressed into a two-dimensional carbon fiber preform prepared in step 1) by a coating method and cross-linked and cured (the curing temperature is 150-300 o C, curing pressure is 0.1-2 MPa, and holding time is 4-8 h); 5) Fix the composite material cured in step 4 with a tool and pyrolyze it in a pyrolysis atmosphere (one of nitrogen, ammonia or argon) according to a specific system (pyrolysis temperature is 900-1400 o C, holding time 2-4 h), to obtain SiCN ceramic-based composite materials with a certain porosity; 6) A liquid SiCN precursor with low viscosity (100-800 mPa·S) is used to impregnate the SiCN ceramic-based composite material with a certain porosity obtained in step 5 under vacuum conditions (0.1 MPa, immersion at room temperature for 2-4 h) and then crack it. The impregnation and cracking cycles are repeated 4-10 times to densify the ceramic-based composite material.

[0028] By adjusting the monomer ratio, a SiCN precursor with controllable side active groups and branching degree was prepared under solvent-free conditions. The prepared SiCN precursor, peroxide initiator, volatile components and active fillers formed a mixed system, which was then composited with a carbon fiber preform containing a cracked carbon layer through a coating method and cured and cracked to form a SiCN ceramic-based composite material with a certain porosity. Subsequently, a low-viscosity SiCN precursor was used as an impregnating agent, and the ceramic-based composite material was densified through several rounds of PIP process.

[0029] The technical effects are as follows: First, a SiCN precursor with controllable side-active groups and branching degree was prepared by adjusting the ratio of chlorosilane monomers, and small molecules and oligomers were removed by vacuum distillation. At the same time, active fillers and volatile components were added to achieve a high ceramic yield while reducing the deformation, shrinkage and cracking of ceramic-based composites. Compared with the ~50% ceramic conversion rate of most precursors, the ceramic conversion rate of the precursor composite system can reach more than 70% due to the synergistic effect of the adjustable side-active groups and branching degree, the addition of active fillers and the removal of small molecules and oligomers. The high ceramic yield makes it possible to achieve the densification of the composite material through a low number of PIP processes, thereby improving the densification efficiency of the composite material and shortening the preparation time.

[0030] By introducing volatile components into the precursor, the occurrence of deformation, shrinkage and cracks can be effectively reduced. The slow pyrolysis or volatilization process of organic components or low-boiling components at lower temperatures can produce fine pores, which is conducive to the release of thermal stress. In addition, since the escape of components can provide a channel for the escape of organic gases in the precursor at high temperatures, it helps to reduce large deformation and cracking, and improve the surface morphology and dimensional accuracy of the final pyrolysis sample. The addition of active fillers can not only make up for the mass loss caused by volatile components, but also fill the pores formed during the pyrolysis of the precursor, so that high ceramic yield can be achieved while reducing the occurrence of system deformation, shrinkage and cracks.

[0031] The coating and impregnating agent used in the SiCN ceramic-based composite material prepared in the embodiment provided by the present invention both use a homemade SiCN precursor, but the composition ratio of the two is different. The price of the monomer and the cross-linking agent is relatively low, and the development cost of other precursors represented by the SiCN precursor is greatly reduced.

[0032] The technical solution of the present invention is further described below through the accompanying drawings and embodiments. Example

[0033] The present invention provides a method for preparing a high-viscosity SiCN precursor, comprising the following steps: Under nitrogen protection, 152.1 g of methylvinyldichlorosilane, 30.9 g of methylhydrogendichlorosilane, 201.1 g of trichloromethylsilane and 837.3 g of hexamethyldisilazane were added in a dry reaction container in sequence, and stirred at room temperature for 30 min without solvent to ensure that the components were fully mixed.

[0034] Subsequently, the reaction system was placed in an oil bath, heated to a slight boiling point, and refluxed for 2 h. After atmospheric distillation, the system was distilled under reduced pressure until no fraction was distilled out, and then naturally cooled to room temperature to obtain a SiCN precursor with high viscosity. The sample had poor fluidity at room temperature after distillation (viscosity was higher than 100,000 mPa·s). Figure 1 This is the thermogravimetric curve of Example 1, and the ceramic yield is 52.9%. Example

[0035] The present invention provides a method for preparing a low-viscosity SiCN precursor, comprising the following steps: Under nitrogen protection, 128 g of methylvinyldichlorosilane, 104.4 g of methylhydrogendichlorosilane, 271.6 g of trichloromethylsilane and 1100.4 g of hexamethyldisilazane were added in a dry reaction container in sequence, and stirred at room temperature for 30 min without solvent to ensure that the components were fully mixed.

[0036] Subsequently, the reaction system was placed in an oil bath, heated to a slight boiling point, and refluxed for 2 h. After atmospheric distillation, the system was distilled under reduced pressure until no fraction was distilled out, and then naturally cooled to room temperature to obtain a SiCN precursor with low viscosity. After distillation, the sample had good fluidity at room temperature (viscosity was less than 1000 mPa·s). Figure 2 This is the thermogravimetric curve of Example 2, and its ceramic yield is 52%. Figure 4 The NMR of Example 2 1 The H spectrum shows the presence of active groups such as vinyl and silicon-hydrogen bonds in the precursor prepared in this example. Example

[0037] The present invention provides a method for preparing a low-viscosity SiCN precursor, comprising the following steps: Under nitrogen protection, 135.43 g of methylvinyldichlorosilane, 104.29 g of trichloromethylsilane and 1162.01 g of hexamethyldisilazane were added in sequence into a dry reaction container, and stirred at room temperature for 30 min without solvent to ensure that the components were fully mixed.

[0038] Subsequently, the reaction system was placed in an oil bath, heated to a slight boiling point, and refluxed for 2 h. After atmospheric distillation, the system was distilled under reduced pressure until no fraction was distilled out, and then naturally cooled to room temperature to obtain a SiCN precursor with low viscosity. After distillation, the sample was solid at room temperature. Figure 3 This is the thermogravimetric curve of Example 3, and the ceramic yield is 69.5%. Example

[0039] The present invention provides a method for preparing a SiCN-based composite material, comprising the following steps: (1) T300-2k twill fabric was used as reinforcement and cut into a rectangle of 80 mm × 120 mm. Pyrolytic carbon was deposited on the surface of the carbon fabric using methane as the gas source at a deposition temperature of 1000 o C. Depositing cracked carbon on the surface of carbon cloth for 4 h can obtain a carbon fiber fabric containing a cracked carbon layer; (2) The high viscosity SiCN precursor, dicumyl peroxide (0.5% of the mass of the precursor) and furan (5% of the mass of the precursor) prepared in Example 1 were dissolved in toluene, and then the active filler Al (average particle size of 2 µm, added in an amount of 10% of the mass of the precursor) was fully dispersed in the precursor mixture system. After the solvent was removed by vacuum rotary evaporation, the precursor mixture system and the carbon cloth containing the cracking layer were layered in a mass ratio of 6:4, with five layers of fiber cloth and five layers of precursor respectively. After the layering was completed, they were hot-pressed and cured on a flat vulcanizer. The curing system was as follows: 120 o C without pressure for 2 h; raise the temperature to 200 o C without pressure for 3 h; raise the temperature to 250 o C, pressure 2 MPa, keep warm for 3 h, and then slowly cool to room temperature.

[0040] (3) The cured SiCN precursor and carbon fiber composite material was fixed with a graphite tool and cracked in a nitrogen atmosphere, and the temperature was gradually raised to 1000 o C isothermal pyrolysis for 3 h, and then gradually cooled to room temperature to obtain SiCN-based carbon fiber composites with certain porosity (unless otherwise specified, the ceramic yields below are all the ceramic yields of the first round of pyrolysis).

[0041] (4) After the SiCN prepared in Example 2 is fully mixed with a diisopropyl peroxide solution (the amount of diisopropyl peroxide added is 0.5% of the mass of the precursor), the SiCN-based carbon fiber composite material obtained in step (3) is immersed in a vacuum condition (0.1 MPa) at room temperature for 4 h, and then cured in an oven and ceramicized according to the pyrolysis system in step (4).

[0042] (5) Repeat step (4) 8-10 times.

[0043] The density of the SiCN ceramic matrix composite material prepared in Example 4 is 1.75 g / cm 3 The ceramic yield after pyrolysis can reach 65%, and the thickness deformation rate of the material is +7.1%. Example

[0044] The present embodiment provides a method for preparing a SiCN-based composite material, which is basically the same as that of Example 4, except that: The high viscosity precursor in step (2) is replaced by a mixed system of SiCN precursors prepared in Example 2 and Example 3, with the ratio of the two being 1:1.

[0045] The density of the SiCN ceramic matrix composite material prepared in Example 5 is 1.79 g / cm 3 The ceramic yield after pyrolysis can reach 79%, and the thickness deformation rate of the material is +5.3%. Example

[0046] The present embodiment provides a method for preparing a SiCN-based composite material, which is basically the same as that of Example 4, except that: In step (2), the active filler is replaced with an inert filler BN (average particle size of 0.3 µm), and the added amount is still 10% of the precursor mass.

[0047] The density of the SiCN ceramic matrix composite material prepared in Example 6 is 1.62 g / cm 3 The ceramic yield after pyrolysis can reach 62%, and the thickness deformation rate of the material is 9.2%. Example

[0048] The present embodiment provides a method for preparing a SiCN-based composite material, which is basically the same as that of Example 4, except that: In step (2), furan was not added, and the active filler was replaced by an inert filler BN (average particle size of 0.3 µm), and the added amount was still 10% of the precursor mass.

[0049] The density of the SiCN-based composite material prepared in Example 7 is 1.68 g / cm 3 The ceramic yield after pyrolysis can reach 57%, and the thickness deformation rate of the material is +15.3%.

[0050] Table 1 Performance indexes of SiCN-based composite materials samples prepared in Examples 4-7 sample Primary pyrolysis ceramic yield / % Initial thickness change rate / % <![CDATA[Density / g / cm 3 <!-- 7 -->]]> Example 4 65 +7.1 1.75 Example 5 79 +5.3 1.79 Example 6 62 +9.2 1.62 Example 7 57 +15.3 1.68 Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application, rather than to limit it. Although the present application has been described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solution described in the above embodiments can still be modified, or some or all of the technical features can be replaced by equivalents. These modifications or replacements are within the scope of protection of the present invention.

Claims

1. A method for preparing a SiCN precursor, characterized in that: The steps include: 1) Add dichlorosilane, trichlorosilane and hexamethyldisilazane into a dry reaction container filled with inert gas, and stir at room temperature for 30 minutes to fully mix the components; wherein the molar ratio of dichlorosilane to trichlorosilane is (1:0)-(1:1), and the molar ratio of the sum of silicon-chlorine bonds in dichlorosilane and trichlorosilane to the silicon-nitrogen bonds in hexamethyldisilazane is (1:1)-(1:2); 2) Heat the reaction system in an oil bath to a slightly boiling state and reflux for 2-6 hours; 3) The unreacted monomers, salts generated during the reaction and precursor oligomers are removed from the above reaction solution by vacuum distillation to obtain a SiCN precursor with side active groups and controllable branching degree.

2. The method for preparing a SiCN precursor according to claim 1, characterized in that: The dichlorosilane is a mixture of one or more of methyl hydrogen dichlorosilane, methyl vinyl dichlorosilane, methyl phenyl dichlorosilane and diphenyl dichlorosilane.

3. A SiCN precursor, characterized in that The SiCN precursor is prepared by the preparation method of the SiCN precursor according to claim 1 or 2.

4. A method for preparing a deformation-controlled ceramic matrix composite material, characterized in that: The steps include: 1) Chemical vapor deposition method was used, with methane as the gas source, at a temperature of 1000 o C, depositing cracked carbon on the surface of the two-dimensional carbon cloth for 2-6 hours to form a two-dimensional carbon fiber preform containing a cracked carbon layer; 2) dissolving the high-viscosity SiCN precursor of claim 3, the peroxide initiator and the volatile components in an organic solvent, and then uniformly dispersing the active filler in the above solution system; 3) Remove the organic solvent introduced in step 2) by vacuum rotary evaporation, the vacuum degree is 10-120Pa, and the temperature is lower than the boiling point of the organic solvent by ~10 o C; 4) The precursor mixed system from which the organic solvent is removed in step 3) is pressed into a mold with the two-dimensional carbon fiber preform prepared in step 1) by a coating method and cross-linked and cured at a curing temperature of 150-300 o C, curing pressure is 0.1-2MPa, and holding time is 4-8h; 5) Fix the composite material cured in step 4) with a tool and pyrolyze it in a pyrolysis atmosphere at a pyrolysis temperature of 900-1400 o C, the holding time is 2-4h, and a SiCN ceramic-based composite material with pores is obtained; 6) A low-viscosity liquid SiCN precursor according to claim 3 is selected as an impregnating agent, and the porous SiCN ceramic-based composite material obtained in step 5) is impregnated at room temperature for 2-4 hours under 0.1 MPa and then cracked, and the impregnation and cracking cycles are 4-10 rounds to densify the ceramic-based composite material.

5. The method for preparing a ceramic-based composite material with controlled deformation according to claim 4, characterized in that: In step 1): The two-dimensional carbon cloth is woven from at least one of T300-grade carbon fiber, T700-grade carbon fiber, T800-grade carbon fiber, T1000-grade carbon fiber and M40J-grade carbon fiber.

6. The method for preparing a ceramic-based composite material with controlled deformation according to claim 4, characterized in that: In step 2): The peroxide initiator is a mixture of one or more of diisopropylbenzene peroxide, benzoyl peroxide, di-tert-butyl peroxide and diisopropylbenzene hydroperoxide.

7. The method for preparing a ceramic-based composite material with controlled deformation according to claim 4, characterized in that: In step 2): The volatile component is one or more of furan, low molecular weight polycarbosilane or low molecular weight polysilazane, and the added amount is 1-8wt.% of the mass of the SiCN precursor.

8. The method for preparing a ceramic-based composite material with controlled deformation according to claim 4, characterized in that: In step 2): The active filler is a mixture of one or more of B, Si, Al, Ti, Mo, CrSi2, MoSi2, AlN, and B4C, and the amount of the active filler added is 1%-10wt.% of the content of the SiCN precursor.

9. The method for preparing a ceramic-based composite material with controlled deformation according to claim 4, characterized in that: In step 5): the cracking atmosphere is one of nitrogen, ammonia and argon.

10. A controlled deformation ceramic matrix composite material, characterized in that: The ceramic matrix composite material is prepared by the method for preparing the controlled deformation ceramic matrix composite material according to any one of claims 4 to 9.

Citation Information

Patent Citations

  • Synthesis of silicon based ceramic forerunner by chloro-silicane hybrid aminolysis modification and preparation method thereof

    CN101139203A

  • Preparation method of Si-C-N ceramic precursor

    CN102660030A

  • Photocured 3D printed polysilazane ceramic product and preparation method thereof

    CN110002883A

  • Ceramic precursor polymer suitable for photocuring molding

    CN116987272A

  • Deformation-controlled ceramic matrix composite material and preparation method thereof