Air-entraining and viscosity-reducing type water reducing agent and synthesis method thereof

Through the non-covalent bonding technology of air-reducing and viscosity-reducing water reducing agent, a gradient side chain structure is formed, which solves the problem of unstable compounding effect of polycarboxylic acid water reducing agent in high-grade concrete, and realizes water reduction and gas extraction The dual role of the concrete improves the fluidity and bubble stabilization performance.

CN118909262APending Publication Date: 2024-11-08黄松
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410959852.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When existing polycarboxylic acid water reducing agents are used in high-grade concrete, it is difficult to achieve stable effect through multi-component compounding, resulting in insufficient long-term and stable performance of concrete, and the types of additives are used in large quantities, which causes heavy production burden.

Method used

采用一种引气降黏型减水剂,通过减水主链与改性侧链的非共价键结合,形成梯度长度的多种侧链,结合苯基辛醇和单辛基酚聚乙二 Alcohol forms hydrophobic and hydrophilic phases, achieving the dual effects of reducing water and evaporating gas.

Benefits of technology

Simplify the composition of concrete, significantly improve the fluidity and apparent air-induced effect of concrete, reduce viscosity, improve the fluidity and bubble stabilization performance of concrete, avoid gas damage, and enhance the support and wetting effect of cement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949954580000131
    Figure BDA0004949954580000131
  • Figure BDA0004949954580000141
    Figure BDA0004949954580000141
  • Figure BDA0004949954580000142
    Figure BDA0004949954580000142
Patent Text Reader

Abstract

The invention relates to the technical field of water reducing agents, and discloses an air-entraining and viscosity-reducing type water reducing agent and a synthesis method thereof in order to solve the problems of heavy production burden and unstable functional effect caused by multiple types of auxiliaries and large dosage, the air-entraining and viscosity-reducing type water reducing agent comprises a water reducing main chain and a modified side chain grafted to the water reducing main chain; the modified side chain comprises a short chain and a long chain, the end part, far away from the main chain, of the long chain is combined with the end part, far away from the main chain, of the short chain through a non-covalent bond, the short chain can be obtained by grafting phenyl octanol to the water-reducing main chain, and the long chain can be obtained by grafting monooctyl phenol polyethylene glycol to the water-reducing main chain. According to the air-entraining and viscosity-reducing type water reducing agent disclosed by the invention, through specific improvement on a molecular chain structure, free water in gaps in a concrete system can be remarkably improved, the viscosity of concrete is reduced, namely, the water reducing effect is improved, and an air-entraining effect can be exerted by constructing a bubble hydrophobic phase at the end part of a side chain.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water reducing agents, and in particular to an air-entraining and viscosity-reducing water reducing agent and a synthesis method thereof. Background Art

[0002] Concrete is mainly composed of sand, gravel, glue and water reducing agent, etc. Among them, the main function of water reducing agent is to improve the workability of concrete, by reducing the amount of water in concrete, thereby improving the strength and durability of concrete, so that concrete can show excellent performance in many aspects such as highway bridges, building structures, underground structures and prefabricated components.

[0003] At present, the common water reducers on the market are mainly divided into aliphatic water reducers and polycarboxylic acid water reducers. Compared with other traditional water reducers, polycarboxylic acid water reducers have outstanding water reduction rate and slump retention, which can give concrete better construction performance, and thus are more widely used. However, polycarboxylic acid water reducers are sensitive to changes in cement and sand materials, so they need to be compounded before use to introduce a variety of functional materials such as viscosity reduction, water retention, and mud resistance to improve the actual adaptability of polycarboxylic acid water reducers.

[0004] For example, the patent with publication number CN115806404A discloses an anti-mud type polycarboxylic acid water reducer, including a polymerization monomer, a polymerization initiator, a molecular weight regulator, a small molecule anti-mud agent, hydrogen peroxide, a chain transfer agent, an air entraining agent, a retarder and a sacrificial agent, etc. By compounding the sacrificial agent with the polycarboxylic acid water reducer, it can also have a certain anti-mud effect and good collapse protection performance.

[0005] However, the existing polycarboxylate water-reducing agent mentioned above is often difficult to achieve the desired effect in actual use only by means of multi-component compounding, especially for high-standard infrastructure such as bridges, high-speed railways, and subways, which usually use high-grade concrete. In the mix ratio of such concrete, the water-cement ratio is low, resulting in high viscosity of the concrete mixture, which has a serious impact and hindrance on construction or pumping. Summary of the invention

[0006] The technical problems to be solved by the present invention are:

[0007] It is often necessary to add a variety of additives with different effects such as retarders, air entraining agents, water reducers, etc. to concrete in order to give the concrete better comprehensive performance. However, the many types of additives added and the large amounts used have caused the problem of heavy production burden. In addition, the mixing and compounding of multiple components will lead to the problem of unstable functional effects of the additives themselves, resulting in the performance of the concrete not being long-lasting and stable enough.

[0008] The technical solution adopted by the present invention is:

[0009] The present invention provides an air-entraining and viscosity-reducing water-reducing agent, comprising a water-reducing main chain and a modified side chain grafted to the water-reducing main chain;

[0010] The modified side chain includes a short chain and a long chain, and the end of the long chain away from the main chain is bonded to the end of the short chain away from the main chain through a non-covalent bond.

[0011] Preferably, the short chain is obtained by grafting phenyloctanol onto a water-reducing backbone.

[0012] Preferably, the long chain is obtained by grafting monooctylphenol polyethylene glycol onto a water-reducing backbone.

[0013] A method for synthesizing the above-mentioned air-entraining viscosity-reducing water-reducing agent comprises the following steps:

[0014] S1 synthetic water-reducing backbone:

[0015] Take maleic anhydride, heat and melt it to obtain a base material;

[0016] Separately take mercaptoethanol and acrylic acid, add them into the solvent, mix, and obtain material A;

[0017] Take styrene separately, add it into the solvent, mix, and obtain material B;

[0018] Add azobisisobutyl cyanide to the base material, stir, then drop material A and material B at the same time, heat to react, and distill to remove the solvent to obtain a water-reducing main chain;

[0019] S2 grafted modified side chain:

[0020] Take the water-reducing main chain, heat it, add phenyloctanol and monooctylphenol polyethylene glycol, add a catalyst, and react; after the reaction is completed, cool it to obtain an air-entraining and viscosity-reducing water-reducing agent.

[0021] Preferably, material A and material B are added dropwise at a uniform speed, and the total addition time is controlled to be 80-100 min.

[0022] Preferably, in step S1, the usage ratio of the base material, the A material and the B material is 1:1.2-1.5:1.5-1.85 by mass.

[0023] Preferably, by mass, the ratio of mercaptoethanol, acrylic acid and solvent in material A is 1:30-40:40-60, and the ratio of styrene to solvent in material B is 1-1.1:1.

[0024] Preferably, in step S1, azobisisobutylcyanide accounts for 1-1.05% of the total mass of reactants for synthesizing the water-reducing backbone.

[0025] Preferably, in step S1, the reaction temperature after dropwise addition of material A and material B is 70-100°C.

[0026] Preferably, in step S2, the heating temperature is 200-220°C and the reaction time is 5-8h.

[0027] The beneficial effects of the present invention are as follows:

[0028] Among conventional concrete additives, it is known that water reducers exert water-reducing effects by acting on the surface of cement particles, while air entraining agents introduce tiny bubbles into concrete to fill the interior of the fluidized concrete, thereby achieving the effects of support and lubrication. Therefore, it is difficult for traditional concrete additives to achieve both water-reducing and air-entraining effects at the same time. The present invention proposes a water-reducing agent with air-entraining effects, which can act as both a water-reducing agent and an air-entraining agent, and can achieve better water-reducing and air-entraining effects while simplifying the composition of concrete.

[0029] The air-entraining and viscosity-reducing water-reducing agent of the present invention has a combing structure required for a water-reducing agent, a main chain of which is a carboxyl anchoring group, and linear side chains are introduced into the main chain by phenyloctanol and monooctylphenol polyethylene glycol. Among them, phenyloctanol, as a side chain, has the characteristics of short chain and strong hydrophobicity; and the side chain formed by monooctylphenol polyethylene glycol is hydrophilic at the end close to the main chain, and the outer end away from the main chain contains a hydrophobic phenylalkyl structure. Phenyloctanol and monooctylphenol polyethylene glycol are connected to the main chain of the water-reducing agent molecule to form a variety of side chains with gradient lengths. The long side chain formed by monooctylphenol polyethylene glycol is easy to bend and deflect, and its terminal hydrophobic group away from the main chain is combined with the short chain group through non-covalent surface tension to form a hydrophobic phase for constructing bubbles; the side chain formed by phenyloctanol is moderate in length, and can provide an excessive effect to compensate for the limited degree of bending and deflection of monooctylphenol polyethylene glycol, and has a good foam stabilizing effect.

[0030] In the air-entraining and viscosity-reducing water-reducing agent of the present invention, the inner side of the side chain close to the main chain is hydrophilic, while the outer side of the side chain away from the main chain is hydrophobic. Such an arrangement feature can make the water-reducing agent molecules form a surrounding bubble structure. These bubbles have an adsorption effect on the cement surface, and can enrich microbubbles on the cement surface to form a certain degree of gas-solid phase, thereby enhancing the supporting and wetting effect of cement, and reducing the adsorption of free water by water, releasing more free water, reducing the unit water consumption of concrete, and improving its fluidity. Especially for high-grade concrete with a low water-cement ratio, the amount of free water is very sensitive to the change of concrete viscosity. The air-entraining and viscosity-reducing water-reducing agent of the present invention can significantly increase the interstitial free water in the concrete system, thereby reducing the viscosity of the concrete, and can provide an outstanding apparent air entraining effect, effectively avoiding the problem of air loss in concrete. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] The invention provides an air-entraining viscosity-reducing water-reducing agent, and the raw materials for preparing the water-reducing agent include: maleic anhydride, acrylic acid, mercaptoethanol, styrene, azobisisobutylcyanide, phenyloctanol, and monooctylphenol polyethylene glycol (OP-60).

[0033] Among them, the structural formula of phenyloctanol is Ph-CH2(CH2)6CH2OH; the structural formula of monooctylphenol polyethylene glycol (OP-60) is HO(CH2CH2O) n -(CH2)8-Ph, where n represents the number of repeating units of the ethylene glycol group and indicates the degree of polymerization of ethylene glycol in the polymer.

[0034] The preparation method of the air-entraining viscosity-reducing water-reducing agent of the present invention comprises the following steps:

[0035] (1) Synthetic water-reducing backbone

[0036] Take maleic anhydride, heat it to 60-70°C, and make it completely melt to obtain the base material;

[0037] Separately, mercaptoethanol and acrylic acid are added to the solvent, mixed, and configured into material A;

[0038] Take styrene separately, add it into the solvent, mix, and prepare material B;

[0039] Add azobisisobutyl cyanide to the completely melted base material, stir, and slowly and uniformly add material A and material B dropwise, both of which are controlled to be added within about 80-100 minutes, heat to 70-100°C, react for 100-150 minutes, and distill to remove the solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0040] Among them, the usage ratio of mercaptoethanol, acrylic acid and solvent in material A is 1:30-40:40-60, the usage ratio of styrene and solvent in material B is 1-1.1:1; the usage ratio of base material, material A and material B is 1:1.2-1.5:1.5-1.85 (by mass); azobisisobutyl cyanide accounts for 1-1.05wt% of the total mass of reactants for synthesizing the water-reducing main chain.

[0041] (2) Grafting modified side chain

[0042] According to the mass fraction, 10 parts of maleic anhydride-styrene copolymer are heated to 200-220°C, 0.8-1.5 parts of phenyloctanol and 2-5 parts of monooctylphenol polyethylene glycol are added, and then 0.3-0.8 parts of catalyst are added, and the mixture is stirred for reaction for 5-8 hours. After the hydroxyl groups of phenyloctanol and monooctylphenol polyethylene glycol are removed, the hydroxyl groups are connected to the main chain of maleic anhydride-styrene copolymer. After the reaction is completed, the mixture is cooled to below 100°C and pure water is added to obtain an air-entraining and viscosity-reducing water-reducing agent.

[0043] In the present invention, the side chains of the water reducer molecule include styrene, phenyloctanol and monooctylphenol polyethylene glycol, etc. Under the action of non-covalent surface tension, the distal end of the long side chain monooctylphenol polyethylene glycol is combined with the distal end of the short side chain styrene to construct a bubble hydrophobic phase, and phenyloctanol can compensate for the excessive effect provided by the long side chain due to the limited bending degree, further construct the bubble hydrophobic phase, and have a good foam stabilizing effect. These bubbles have an adsorption effect on the cement surface, can enrich microbubbles on the cement surface, and form a certain degree of gas-solid phase, thereby enhancing the supporting and wetting effect of the cement.

[0044] Example 1

[0045] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C to completely melt it, and obtain a base liquid; take another 1.5 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0046] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0047] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 6 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0048] Example 2

[0049] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0050] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0051] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 6 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0052] Example 3

[0053] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2.5 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0054] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0055] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 6 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0056] Example 4

[0057] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 50 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0058] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0059] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 6 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0060] Example 5

[0061] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 80 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0062] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0063] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 6 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0064] Example 6

[0065] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 110 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add it to 100 parts of toluene, stir and mix, and obtain material B.

[0066] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0067] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 6 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0068] Example 7

[0069] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0070] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0071] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, and then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 5 hours, cool to below 100°C, and add 30 parts of pure water to obtain an air-entraining and viscosity-reducing water-reducing agent.

[0072] Example 8

[0073] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0074] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0075] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 3 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 7 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0076] Example 9

[0077] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0078] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0079] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 2.2 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 7 hours, cool to below 100°C, add 30 parts of pure water, and obtain an air-entraining and viscosity-reducing water-reducing agent.

[0080] Example 10

[0081] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0082] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0083] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 1 part of 8-phenyloctanol and 5 parts of monooctylphenol polyethylene glycol, and then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 7 hours, cool to below 100°C, and add 30 parts of pure water to obtain an air-entraining and viscosity-reducing water-reducing agent.

[0084] Comparative Example 1

[0085] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0086] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0087] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 4 parts of monooctylphenol polyethylene glycol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 7 hours, cool to below 100°C, add 30 parts of pure water, and obtain a water reducer.

[0088] Comparative Example 2

[0089] Step 1: Take 120 parts of maleic anhydride by mass, add it to a three-necked flask, heat it to about 65°C, and completely melt it to obtain a base liquid; take another 2 parts of mercaptoethanol and 70 parts of acrylic acid, add them to 100 parts of toluene, stir and mix, and obtain material A; take another 105 parts of styrene, add them to 100 parts of toluene, stir and mix, and obtain material B.

[0090] Step 2: Add 0.5 parts of azobisisobutyl cyanide to the completely melted base liquid, stir for about 5 minutes to mix it, then add material A and material B at a uniform speed, control the dripping to be completed within 90 minutes, heat to 80°C, react for 120 minutes, and then distill off the toluene solvent to obtain a carboxyphenyl-rich maleic anhydride-styrene copolymer.

[0091] Step 3: Take 10 parts of maleic anhydride-styrene copolymer by mass, heat to 200°C, add 4 parts of 8-phenyloctanol, then add 0.5 parts of p-aminobenzenesulfonic acid, stir and react for 7 hours, cool to below 100°C, add 30 parts of pure water, and obtain a water reducer.

[0092] Test example

[0093] Samples: Examples 1-10 and Comparative Examples 1-2 (one)

[0095] The water reducing agent samples of Examples 1-10 and Comparative Examples 1-2 were respectively used in concrete, and mixed at a ratio of cement: water: water reducing agent = 300: 87: 0.5 (by mass) to prepare concrete slurry, and the net slurry fluidity of the concrete slurry was tested. The structures are summarized in Table 1 below:

[0096] Table 1 Test results of concrete slurry fluidity using different water reducing agent samples

[0097]

[0098]

[0099] It can be seen from Table 1 above that the water reducing agent prepared by Examples 1 to 10 is applied to concrete slurry, and its fluidity is more durable and stable, and the effect is better under the dosage ratio and preparation conditions of Example 8. (two)

[0101] The air-entraining and viscosity-reducing water-reducing agent, polycarboxylic acid water-reducing agent, and the combination of polycarboxylic acid water-reducing agent and air-entraining agent in Example 8 were respectively used, and cement: fly ash: sand: stone: water = 340:80:835:980:165 (by mass) were mixed to prepare concrete slurry, and its slump retention performance was tested. The results are summarized in the following Table 2:

[0102] Table 2 Concrete slurry performance test results of different water reducing agent samples

[0103]

[0104] It can be seen from Table 2 that the combination of traditional polycarboxylic acid water-reducing agent and air-entraining agent can significantly reduce the viscosity of concrete and adjust the state of concrete, but its effect gradually weakens over time. The air-entraining and viscosity-reducing water-reducing agent in Example 8 can still maintain a low viscosity after a certain period of time, thereby improving the durability and stability of the water-reducing and air-entraining effects. (three)

[0106] Take 80mL of water and 20mL of air-entraining viscosity-reducing water-reducing agent and place them in a 200mL measuring cylinder. Shake and oscillate to generate bubbles and observe the volume of the bubbles. Repeat the shaking and oscillating operation until the bubbles are highly stable. Measure the volume of the bubbles. After standing, measure the volume of the bubbles again to reflect the stability of the bubbles. The results are summarized in Table 3 below:

[0107] Table 3 Foam stabilization test results of different water reducing agent samples

[0108] Comparison Items Initial bubble volume Bubble volume after 60min of static Bubble volume after 120min of static Example 9 60 20 12 Example 10 55 49 41 Comparative Example 1 17 8 2

[0109] It can be seen from Table 3 that when the dosage ratio of 8-phenyloctanol and monooctylphenol polyethylene glycol changes, the volume of bubbles generated and the stability of the bubble volume will be significantly affected. When the dosage of 8-phenyloctanol and monooctylphenol polyethylene glycol specified in the present invention is used, a large number of bubble structures can be generated by reaction, and after standing for a certain period of time, a relatively high amount of bubbles is still maintained, which means that the air-entraining and viscosity-reducing water-reducing agent in the present invention can not only exert a good water-reducing effect, but also support and lubricate the cement-based material through the bubble structure.

[0110] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An air-entraining viscosity-reducing water-reducing agent, characterized in that: It includes a water-reducing main chain and a modified side chain grafted to the water-reducing main chain; The modified side chain includes a short chain and a long chain, and the end of the long chain away from the main chain is bonded to the end of the short chain away from the main chain through a non-covalent bond.

2. The air-entraining viscosity-reducing water-reducing agent according to claim 1, characterized in that: The short chain is obtained by grafting phenyloctanol onto the water-reducing main chain.

3. The air-entraining viscosity-reducing water-reducing agent according to claim 1 or 2, characterized in that: The long chain is obtained by grafting monooctylphenol polyethylene glycol onto the water-reducing main chain.

4. A method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to any one of claims 1 to 3, characterized in that: The steps include: S1 synthetic water-reducing backbone: Take maleic anhydride, heat and melt it to obtain a base material; Separately take mercaptoethanol and acrylic acid, add them into the solvent, mix, and obtain material A; Take styrene separately, add it into the solvent, mix, and obtain material B; Add azobisisobutyl cyanide to the base material, stir, then drop material A and material B at the same time, heat to react, and distill to remove the solvent to obtain a water-reducing main chain; S2 grafted modified side chain: Take the water-reducing main chain, heat it, add phenyloctanol and monooctylphenol polyethylene glycol, add a catalyst, and react; after the reaction is completed, cool it to obtain an air-entraining and viscosity-reducing water-reducing agent.

5. The method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to claim 4, characterized in that: Add material A and material B at the same time at a uniform speed, and control the total addition time to be 80-100 minutes.

6. The method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to claim 5, characterized in that: In step S1, the usage ratio of the base material, the A material and the B material is 1:1.2-1.5:1.5-1.85 by mass.

7. The method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to claim 4, characterized in that: By mass, the ratio of mercaptoethanol, acrylic acid and solvent in material A is 1:30-40:40-60, and the ratio of styrene to solvent in material B is 1-1.1:

1.

8. The method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to claim 4, characterized in that: In step S1, azobisisobutylcyanide accounts for 1-1.05 wt% of the total mass of reactants for synthesizing the water-reducing backbone.

9. The method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to claim 4, characterized in that: In step S1, the reaction temperature after the dropwise addition of material A and material B is 70-100°C.

10. The method for synthesizing the air-entraining viscosity-reducing water-reducing agent according to claim 4, characterized in that: In step S2, the heating temperature is 200-220°C and the reaction time is 5-8h.

Citation Information