Additive manufacturing composite material and preparation method and application thereof
By using specific formulas and process designs of components such as hollow microbeads and thermoplastic resins in additive manufacturing composite materials, a unique network support structure is formed, which solves the problem of improving the performance of existing materials, and achieves mechanical properties, heat resistance and The corrosion resistance is significantly improved and is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202411139853.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new material technology, and in particular to an additive manufacturing composite material and a preparation method and application thereof. Background Art
[0002] With the rapid development of science and technology, additive manufacturing technology (3D printing technology), as an important branch of advanced manufacturing technology, has shown great application potential and value in many fields. Traditional material preparation and processing methods are often limited by the difficulty of balancing material properties. However, additive manufacturing technology has successfully broken these constraints with its unique layer-by-layer additive molding method, paving a new path for the innovative design and manufacturing of composite materials.
[0003] At the same time, additive manufacturing composite materials not only cleverly integrate the superior properties of multiple materials and realize personalized customization of material performance, but also achieve fine-grained regulation at the microstructure level, thereby greatly improving the overall performance of the material. In recent years, with the close integration of materials science and computer technology, the types of additive manufacturing composite materials have become increasingly diverse, and their application scope has also shown a trend of continuous expansion.
[0004] Although additive manufacturing composite materials have achieved remarkable achievements in material design and processing technology, how to further optimize the mechanical properties, heat resistance, corrosion resistance and long-term stability of the materials is still a hot and difficult issue that scientific researchers are eager to overcome. Summary of the invention
[0005] In view of this, the present invention proposes an additive manufacturing composite material and a preparation method and application thereof, aiming to further promote breakthroughs in the application of additive manufacturing composite materials in fields requiring high performance through innovative material formulations and unique process designs.
[0006] The present invention provides a method for preparing a composite material by additive manufacturing, comprising the following steps: The hollow microspheres are stirred at a temperature of 100-120° C., and when the temperature drops to 50-60° C., thermoplastic resin and distilled water are added and continued to be stirred, and then surfactant and color powder are added and stirred evenly, and finally a film-forming agent is added and continued to be stirred until uniform, and the additive manufacturing composite material is obtained after cooling.
[0007] Preferably, the hollow microspheres are one or more of hollow silica microspheres, hollow titanium dioxide microspheres, hollow glass microspheres, hollow ceramic microspheres, phenolic resin hollow microspheres, calcium carbonate hollow microspheres and polystyrene hollow microspheres.
[0008] Preferably, when the hollow microbeads are hollow silica microbeads, hollow titanium dioxide microbeads, hollow glass microbeads, hollow ceramic microbeads, phenolic resin hollow microbeads, calcium carbonate hollow microbeads and polystyrene hollow microbeads, the weight ratio of the hollow silica microbeads, hollow titanium dioxide microbeads, hollow glass microbeads, hollow ceramic microbeads, phenolic resin hollow microbeads, calcium carbonate hollow microbeads and polystyrene hollow microbeads is 2-3: 1-2: 1-1.5: 1-1.5: 0.5-1: 0.5-1: 0.5-1.
[0009] Preferably, the weight ratio of the hollow silica microbeads, hollow titanium dioxide microbeads, hollow glass microbeads, hollow ceramic microbeads, phenolic resin hollow microbeads, calcium carbonate hollow microbeads and polystyrene hollow microbeads is 2.5:1.5:1.5:1:1:1:0.5.
[0010] Preferably, the thermoplastic resin is one or more of polypropylene, polyethylene, acrylonitrile-butadiene-styrene or copolymers thereof.
[0011] Preferably, the surfactant is one or more of coconut oil, nutmeg, stearic acid, palmitic acid, oleic acid, lauric acid, coconut amine, sodium stearate, sodium laurate, and sodium oleate.
[0012] Preferably, the film-forming agent is one or more of polyvinyl alcohol, lithium silicate, dodecyl alcohol ester and polysiloxane film-forming agents.
[0013] Preferably, the weight ratio of thermoplastic resin, distilled water, surfactant, color powder and film-forming agent is 5-10: 1-5: 0.05-0.1: 0.1-1: 0.1-0.5.
[0014] The present invention also provides an additive manufacturing composite material, which is prepared by the above-mentioned preparation method.
[0015] The present invention also provides an application of the above-mentioned additive manufacturing composite material, and the application includes at least one of the following: A1) Application in environmentally friendly materials; A2) Application in medical devices; A3) Application in building materials; A4) Application in toy materials.
[0016] Compared with the prior art, the present invention has the following beneficial effects: Significantly improve material performance: Through the carefully designed material formula and unique preparation process, the additive manufacturing composite material prepared by the present invention has shown significant improvements in mechanical properties, heat resistance, corrosion resistance and long-term stability. This is mainly due to the introduction of hollow microspheres, which can not only effectively reduce material density and improve the level of lightweight, but also form a unique network support in the microstructure to enhance the overall strength and toughness of the material.
[0017] Enhanced customization capability: The preparation method provided by the present invention allows researchers to flexibly adjust the type and proportion of hollow microspheres, as well as the proportion of thermoplastic resin, surfactant, color powder, film-forming agent and other components according to specific needs, thereby achieving personalized customization of material properties. This high degree of customizability provides a solid foundation for the application of additive manufacturing composite materials in a wider range of fields. DETAILED DESCRIPTION
[0018] The exemplary embodiments of the present disclosure will be described in more detail below. Although the exemplary embodiments of the present disclosure are shown below, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to be able to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0019] Example 1 Preparation of hollow microspheres 1. Hollow silica microbeads Sol-Gel Method: Raw materials: silicate solution (tetraethoxysilane TEOS, concentration 0.5M), catalyst (ammonia water or acidic catalyst, added amount is 0.1% of silicate solution), water.
[0020] Process: Mix silicate solution with water to form silica sol, adjust pH and temperature to gel the sol to form hollow silica spheres, and then calcine to remove organic components to obtain hollow silica microspheres.
[0021] 2. Hollow Titanium Dioxide Microbeads Chemical Vapor Deposition (CVD): Raw materials: tetrabutyl titanate (TBT, concentration 0.5M), oxygen, and nitrogen (used to carry reaction gas).
[0022] Process: Titanium dioxide precursor reacts in the high-temperature gas phase and deposits on the substrate surface to form hollow microspheres.
[0023] 3. Hollow glass microspheres Flotation method: Raw materials: glass raw materials (70 parts by weight of silica sand, 15 parts by weight of sodium alkali, 5 parts by weight of limestone), foaming agent (sodium bicarbonate, the addition amount is 0.5% of the weight of the glass raw materials).
[0024] Process: The glass material is heated to a high temperature and cooled in a controlled environment to form a hollow structure.
[0025] 4. Hollow Ceramic Microspheres Sintering method: Raw materials: ceramic powder (40 parts by weight of kaolin, 30 parts by weight of feldspar, 10 parts by weight of quartz), foaming agent (starch or organic additive, added in an amount of 2 parts by weight).
[0026] Process: Mix powder and foaming agent, and sinter at high temperature to make the foaming agent gas form a hollow structure in the ceramic matrix.
[0027] 5. Phenolic resin hollow microspheres Chemical foaming method: Raw materials: phenolic resin (concentration 30%), foaming agent (ammonium chloride, added amount is 2% of the weight of phenolic resin).
[0028] Process: A blowing agent is added during the resin synthesis process, and the blowing agent releases gas to form hollow microspheres when the resin solidifies.
[0029] 6. Calcium carbonate hollow microspheres Chemical precipitation method: Raw materials: calcium chloride solution (concentration 0.5M), sodium carbonate solution (concentration 0.5M), additives (surfactant, added amount is 0.1% of the weight of calcium chloride solution).
[0030] Process: The two solutions react to form calcium carbonate precipitate, and the conditions are adjusted to form hollow microspheres.
[0031] 7. Polystyrene hollow microspheres Suspension polymerization method: Raw materials: styrene monomer (concentration 10%), foaming agent (nitrogen or carbon dioxide, added in an amount of 5% of the weight of styrene monomer), initiator (persulfate, concentration 0.1%).
[0032] Process: Monomers are mixed with blowing agents, suspended and polymerized to form microspheres, and heated to release gas from the blowing agent to form a hollow structure. Example
[0033] A method for preparing an additively manufactured composite material, comprising: 1. Experimental steps 1. Sample preparation: Eight different sets of cenosphere combination samples were prepared, each set of samples contained a specific type of cenospheres, and the specific groups were as follows: Sample A: Contains only hollow silica microbeads.
[0034] Sample B: Contains only hollow titanium dioxide microspheres.
[0035] Sample C: Contains only hollow glass microspheres.
[0036] Sample D: Contains only hollow ceramic microspheres.
[0037] Sample E: Contains only phenolic resin hollow microspheres.
[0038] Sample F: Contains only calcium carbonate hollow microspheres.
[0039] Sample G: Contains only polystyrene hollow microspheres.
[0040] Sample H: hollow silica microbeads, hollow titanium dioxide microbeads, hollow glass microbeads, hollow ceramic microbeads, phenolic resin hollow microbeads, calcium carbonate hollow microbeads, and polystyrene hollow microbeads are mixed in a specific weight ratio (2.5:1.5:1.5:1:1:1:0.5).
[0041] 2. Surface treatment: A uniform surface treatment process is performed on all types of cenospheres, including but not limited to acid washing, to ensure the consistency of the microsphere surface properties.
[0042] 3. Mixing preparation: The surface treated microbeads were added one by one into the kneader.
[0043] Stirring is performed at a controlled temperature of 100-120°C to ensure that the microbeads are evenly heated and preliminarily mixed.
[0044] Add the corresponding materials according to the established ratio (200 parts of thermoplastic resins PP and PE, 50 parts of distilled water) and continue stirring.
[0045] Add surfactant (0.1 part of stearic acid, 0.05 part of coconut amine), color powder (0.5 part of titanium dioxide) and film former (1 part of polyvinyl alcohol, 0.5 part of polysiloxane) gradually and evenly, while keeping stirring until all ingredients are mixed evenly.
[0046] Finally, a slow cooling method is used to ensure that the mixture remains in a uniform state during the cooling process to prevent internal stress or structural changes, and the additively manufactured composite material is obtained after cooling to room temperature.
[0047] Test Example 1 1. Performance testing of the additively manufactured composite material prepared in Example 2 1. Mechanical properties evaluation First, the tensile strength test was performed on samples A to H. The test was performed using a universal material testing machine in accordance with the ASTM D638 standard, and key parameters such as tensile strength and elongation at break of each sample were recorded. Special attention was paid to sample H, which was a composite material mixed with multiple hollow microspheres, to observe whether it exhibited better mechanical properties than a single microsphere sample, such as whether it exhibited a higher balance between strength and toughness.
[0048] 2. Thermal stability analysis Next, the thermal stability of the samples was evaluated using a thermogravimetric analyzer (TGA) and a differential scanning calorimeter (DSC). The test temperature range was set from room temperature to 800°C, with a heating rate of 10°C / min. The mass loss, thermal decomposition temperature, and thermal transition behavior of each sample during the heating process were analyzed to evaluate the effects of the type and mixing ratio of hollow microspheres on the thermal stability of the composite material.
[0049] 3. Density and porosity measurement The density of each sample was measured by gas expansion method or water displacement method, and its porosity was estimated by theoretical calculation or microscopic observation. The contribution of different hollow microspheres and their combinations to the density and porosity of the composite material was compared, and the mechanism of the influence of pore structure on material properties was explored.
[0050] 4. Sound insulation and heat insulation performance test Given the special structure of hollow microspheres, it is particularly important to test the sound insulation and heat insulation performance of the samples. The sound attenuation ability of the samples was tested using a soundproof chamber, and the thermal conductivity was evaluated using the hot box method. The focus was on the comprehensive performance of sample H in sound insulation and heat insulation, exploring the potential of mixed hollow microspheres in improving the functionality of materials.
[0051] 5. Microstructure observation Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) were used to observe the microstructure of each sample, especially the morphology and distribution of hollow microspheres and the interface bonding between microspheres and the matrix. The effects of different preparation methods on the morphology of microspheres and the microstructure of composite materials were analyzed to provide a theoretical basis for optimizing the preparation process.
[0052] 6. Environmental adaptability test Considering the various environmental conditions that composite materials may face in practical applications, such as humidity, pH, etc., the environmental adaptability test was carried out on the samples. After the samples were placed in an environment with different humidity (20%, 50%, 80%RH) and pH values (3, 7, 11) for a certain period of time, their mechanical properties, appearance, etc. were evaluated to see if they changed, so as to evaluate their environmental stability and durability.
[0053] 7. Additive Manufacturing Application Evaluation Finally, combined with the characteristics of additive manufacturing technology (such as 3D printing), the printing performance of the samples was evaluated. The key indicators of different hollow microsphere composite materials in the 3D printing process, such as fluidity, molding accuracy, and interlayer bonding strength, were tested. The potential applications of hybrid hollow microsphere composite materials in the field of additive manufacturing, such as lightweight structural parts and functional gradient materials, were explored.
[0054] 2. Evaluation Results 1. Mechanical properties evaluation The tensile strength test results show that sample H (a composite material mixed with multiple hollow microspheres) exhibits significant advantages in both tensile strength and elongation at break. Compared with single microsphere samples, sample H not only has higher strength, but also maintains good toughness, achieving a good balance between strength and toughness. This result verifies the effectiveness of the mixed hollow microsphere strategy in improving the mechanical properties of composite materials. In addition, the synergistic effect between different hollow microspheres may also play a positive role in improving mechanical properties.
[0055] 2. Thermal stability analysis Thermogravimetric analysis and differential scanning calorimetry analysis show that the thermal stability of sample H is also better than that of the single microsphere sample. Its thermal decomposition temperature is higher and the mass loss rate is slower, indicating that the mixed hollow microsphere composite material has better stability in high temperature environment. This feature is particularly important for applications that need to work under high temperature conditions.
[0056] 3. Density and porosity measurement The gas expansion method and the drainage method showed that the density of sample H was relatively low, while the porosity was high. This was mainly due to the lightweight characteristics of the hollow microspheres and their internal hollow structure. Mixing multiple hollow microspheres further reduced the density of the composite material while maintaining a high porosity, providing strong support for the application of the material in the field of lightweighting.
[0057] 4. Sound insulation and heat insulation performance test The results of the soundproof room test and the hot box test showed that sample H performed well in terms of sound insulation and heat insulation. Its sound attenuation and thermal conductivity were better than those of the single microbead sample, showing the great potential of mixed hollow microbead composite materials in improving material functionality. This excellent sound insulation and heat insulation performance makes the composite material have a wide range of application prospects in the fields of construction, transportation, etc.
[0058] 5. Microstructure observation SEM and TEM observations reveal the complexity of the microstructure of the hybrid hollow microsphere composite material. The hollow microspheres are evenly distributed in the matrix, with different morphologies but supporting each other, forming a unique network structure. The interface between the microspheres and the matrix is tightly bonded, with no obvious defects or cracks. This microstructure not only helps to improve the mechanical properties of the material, but also provides a physical basis for the material's functionality such as sound insulation and heat insulation.
[0059] 6. Environmental adaptability test The results of the environmental adaptability test show that sample H exhibits good stability and durability under different humidity and pH environments. Its mechanical properties and appearance have not changed significantly, indicating that the hybrid hollow microsphere composite material has good environmental adaptability and can meet the complex and changing practical application needs.
[0060] 7. Additive Manufacturing Application Evaluation In the additive manufacturing application evaluation, sample H showed excellent printing performance. It has good fluidity, high molding accuracy, and strong interlayer bonding strength, making it very suitable for additive manufacturing technologies such as 3D printing. The application potential of hybrid hollow microsphere composite materials in lightweight structural parts and functional gradient materials has been further verified.
[0061] In summary, the additive manufacturing composite materials mixed with various hollow microspheres have excellent performance in mechanical properties, thermal stability, density and porosity, sound insulation and heat insulation performance, and environmental adaptability. This composite material not only has excellent physical properties, but also has broad application prospects and market value. In the future, with the continuous optimization of the preparation process and the continuous expansion of application fields, mixed hollow microsphere composite materials are expected to play an important role in more fields.
[0062] 3. Principle and Mechanism In order to deeply understand the excellent performance of composite materials with mixed hollow microspheres, the following is a detailed analysis of the reasons for the performance improvement: 1. Mechanical performance improvement mechanism: Synergistic effect: The mixed hollow microspheres not only play their own reinforcing role in the composite material, but also improve the overall performance through synergistic effect. The differences in shape, size and mechanical properties of different microspheres enable them to support the matrix in different directions, thereby improving the tensile strength and elongation at break of the composite material.
[0063] Interface bonding: Good interface bonding between microspheres and the matrix is the key to the mechanical properties of composite materials. Hybrid hollow microspheres may form a more complex interface structure during the preparation process, which enhances the interaction between microspheres and the matrix, thereby improving the overall strength of the material.
[0064] 2. Thermal stability enhancement mechanism: Thermal barrier effect: The hollow structure of hollow microspheres provides an additional thermal barrier for the composite material, slowing down the transfer of heat to the inside of the matrix. After mixing multiple hollow microspheres, this thermal barrier effect is more significant, thereby increasing the thermal decomposition temperature and thermal stability of the composite material.
[0065] Differences in pyrolysis behavior: Different types of hollow microspheres have different pyrolysis behaviors. Mixed use can slow down the overall pyrolysis rate to a certain extent, reduce mass loss, and further improve thermal stability.
[0066] 3. Density and porosity optimization mechanism: Lightweight properties: Hollow microspheres themselves have lightweight properties, and mixing multiple hollow microspheres can further reduce the density of the composite material. At the same time, the hollow structure inside the microspheres provides additional pore space for the material, increasing the porosity.
[0067] Structural optimization: By rationally designing the mixing ratio and preparation process, the internal structure of the composite material can be optimized to make the pore distribution more uniform, further improving the lightweight effect and porosity of the material.
[0068] 4. Mechanism for improving sound insulation and heat insulation performance: Sound wave scattering and absorption: The complex structure of the mixed hollow microspheres helps to scatter and absorb sound waves, reduce the transmission and reflection of sound waves, and thus improve the sound insulation performance of the material.
[0069] Heat conduction barrier: The hollow structure and low thermal conductivity of hollow microspheres hinder the conduction of heat in the composite material, reducing the thermal conductivity of the material and improving the thermal insulation performance.
[0070] Interface thermal resistance: The interface thermal resistance between microspheres and the matrix is also an important factor affecting the thermal insulation performance of the material. Mixing hollow microspheres may increase the interface thermal resistance and further reduce the heat conduction efficiency.
[0071] 5. Environmental adaptability mechanism: Chemical stability: The components in the hybrid hollow microsphere composite material may have good chemical stability and can maintain stable performance under different humidity and pH environments.
[0072] Physical barrier: The structure of hollow microspheres provides an additional physical barrier for the matrix, reducing the erosion and damage of the matrix by external environmental factors.
[0073] 6. Additive manufacturing application mechanism: Flowability and formability: Composite materials mixed with hollow microspheres show good flowability during the additive manufacturing process, which is conducive to uniform distribution and precise forming of materials.
[0074] Interlayer bonding: Reasonable mixing ratio and preparation process can help enhance the interlayer bonding strength and improve the overall performance and service life of the composite material.
[0075] In summary, the reason why additive manufacturing composite materials mixed with multiple hollow microspheres show such excellent performance is mainly due to the synergistic effect between the components, the complex microstructure, and the reasonable preparation process design. These mechanisms work together on the composite materials, making them perform well in many aspects and have broad application prospects and market value.
[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing an additively manufactured composite material, It is characterized in that The following steps are involved: The hollow microspheres are stirred at a temperature of 100-120° C., and when the temperature drops to 50-60° C., thermoplastic resin and distilled water are added and continued to be stirred, and then surfactant and color powder are added and stirred evenly, and finally a film-forming agent is added and continued to be stirred until uniform, and the additive manufacturing composite material is obtained after cooling.
2. The method for preparing a composite material by additive manufacturing according to claim 1, It is characterized in that The hollow microspheres are one or more of hollow silica microspheres, hollow titanium dioxide microspheres, hollow glass microspheres, hollow ceramic microspheres, phenolic resin hollow microspheres, calcium carbonate hollow microspheres and polystyrene hollow microspheres.
3. The method for preparing a composite material by additive manufacturing according to claim 1, It is characterized in that When the hollow microbeads are hollow silica microbeads, hollow titanium dioxide microbeads, hollow glass microbeads, hollow ceramic microbeads, phenolic resin hollow microbeads, calcium carbonate hollow microbeads and polystyrene hollow microbeads, the weight ratio of the hollow silica microbeads, hollow titanium dioxide microbeads, hollow glass microbeads, hollow ceramic microbeads, phenolic resin hollow microbeads, calcium carbonate hollow microbeads and polystyrene hollow microbeads is 2-3: 1-2: 1-1.5: 1-1.5: 0.5-1: 0.5-1: 0.5-1.
4. The method for preparing a composite material by additive manufacturing according to claim 1, It is characterized in that The thermoplastic resin is one or more of polypropylene, polyethylene, acrylonitrile-butadiene-styrene or copolymers thereof.
5. The method for preparing a composite material by additive manufacturing according to claim 1, It is characterized in that The surfactant is one or more of coconut oil, nutmeg, stearic acid, palmitic acid, oleic acid, lauric acid, coconut amine, sodium stearate, sodium laurate, and sodium oleate.
6. The method for preparing a composite material by additive manufacturing according to claim 1, It is characterized in that The film-forming agent is one or more of polyvinyl alcohol, lithium silicate, dodecyl alcohol ester and polysiloxane film-forming agents.
7. The method for preparing a composite material by additive manufacturing according to claim 1, It is characterized in that The weight ratio of the thermoplastic resin, distilled water, surfactant, color powder and film-forming agent is 5-10:1-5:0.05-0.1:0.1-1:0.1-0.
5.
8. An additively manufactured composite material, It is characterized in that The additively manufactured composite material is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the additive manufacturing composite material according to claim 8, It is characterized in that The application includes at least one of the following: A1) Application in environmentally friendly materials; A2) Application in medical devices; A3) Application in building materials; A4) Application in toy materials.