Polymer-assisted stripping boron nitride nanosheet / aramid nanofiber composite heat-conducting film and preparation method thereof
Hexagonal boron nitride is dispersed in CMC and HEC aqueous solutions through polymer-assisted peeling technology to prepare boron nitride nanosheets with high horizontal and aspect ratio and low defects. Combined with aramid nanofibers to form a composite thermal conductive film, solving the existing boron nitride nanometers The problem of insufficient thermal conductivity of sheet-based thermal conductivity films has significantly improved the thermal conductivity.
Patent Information
- Application Number
- CN202411212810.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The thermal conductivity of the existing boron nitride nanosheet-based thermal conductivity films is poor, mainly due to the presence of many lattice defects and functional group intervention during the preparation process, resulting in poor thermal conductivity.
Using polymer-assisted peeling method, hexagonal boron nitride is dispersed in CMC and HEC aqueous solutions. By adjusting the concentration and pressure of the polymer aqueous solution, the degree of coating and shear force of h-BN are changed to prepare a high horizontal and aspect ratio and low The defective boron nitride nanosheets are combined with aramid nanofibers to form a composite thermally conductive film.
The intrinsic thermal conductivity of boron nitride nanosheets and the total thermal conductivity of the composite film are improved, the heat transfer ability is enhanced, and the problem of insufficient thermal conductivity is solved.
Smart Images

Figure CN118909286A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of thermally conductive films, and in particular relates to a polymer-assisted peeled boron nitride nanosheet / aramid nanofiber composite thermally conductive film and a preparation method thereof. Background Art
[0002] The high integration and high power of electronic devices lead to the accumulation of heat in electronic devices, which makes it difficult to dissipate heat, seriously endangering the performance and service life of electronic devices. In order to effectively assist the heat dissipation of electronic devices, people have begun to prepare various insulating thermal conductive materials for heat conduction. In recent years, two-dimensional materials have attracted the attention of technicians due to their excellent physical and chemical properties. Fillers with high thermal conductivity are used to fill the film-forming material to prepare films with high insulation and high thermal conductivity for heat transfer.
[0003] Boron nitride (BN) has excellent chemical and thermal stability, insulation, wave transmission, low dielectric, low density, easy modification, processing, can be composited with polymers, and is a ceramic material with the highest thermal conductivity. Therefore, it is an excellent insulating thermal conductive filler. Combined with a polymer substrate to form a composite thermal conductive film, it has become one of the important ways to solve the auxiliary heat dissipation of electronic devices and has developed rapidly in the field of insulating thermal conductive materials. According to relevant reports, when the thickness of hexagonal boron nitride (h-BN) reaches a single layer or multiple layers, boron nitride nanosheets (BNNS) can better demonstrate its excellent performance in all aspects. However, there are some problems in the BN peeling process, such as the prepared BNNS has more lattice defects, introduces new functional groups, and cannot have a larger aspect ratio, resulting in poor thermal conductivity of the current boron nitride nanosheet-based thermal conductive film.
[0004] In order to improve the thermal conductivity of boron nitride nanosheet-based thermal conductive films, it is necessary to ensure that BNNS can better demonstrate the excellent performance of BN and reduce the involvement of lattice defects and functional groups in the preparation of BNNS. However, among the current methods of stripping BN, the BNNS obtained by ball milling stripping, liquid phase ultrasound, surface activation and interlayer volume expansion methods are small in size, high in thickness, and small in aspect ratio, and still have many lattice defects, which are easy to introduce new functional groups, which is not conducive to the subsequent preparation of high-performance boron nitride nanosheet-based thermal conductive films. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film and a preparation method thereof. h-BN is introduced into a CMC aqueous solution and a HEC aqueous solution, and the h-BN is exfoliated under a certain pressure. The coating degree of the h-BN can be changed by changing the viscosity, thereby changing the collision force and shear force of the h-BN on the homogenization channel during the homogenization process, preparing a BNNS with a high aspect ratio and low defects, improving the intrinsic thermal conductivity of the BNNS, and finally improving the thermal conductivity of the boron nitride nanosheet / aramid nanofiber composite film.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film comprises the following steps:
[0008] S1, dispersing hexagonal boron nitride into a sodium carboxymethyl cellulose aqueous solution, wherein the mass ratio of sodium carboxymethyl cellulose to deionized water in the sodium carboxymethyl cellulose aqueous solution is (0.5-1.5):100, to obtain a first suspension;
[0009] Dispersing hexagonal boron nitride in a hydroxyethyl cellulose aqueous solution, wherein the mass ratio of hydroxyethyl cellulose to deionized water in the hydroxyethyl cellulose aqueous solution is (0.5-1.5):100, to obtain a second suspension;
[0010] S2, homogenizing the first suspension at 75-90 MPa, and then separating the sodium carboxymethyl cellulose therein to obtain a first dispersion;
[0011] homogenizing the second suspension at 75-90 MPa, and then separating the hydroxyethyl cellulose therein to obtain a second dispersion;
[0012] S3, respectively mixing the first dispersion and the second dispersion with the aramid nanofiber dispersion, wherein the aramid nanofiber is a polymer matrix, and the boron nitride nanosheets in the dispersion are thermally conductive fillers, and then performing a film-forming process to obtain a boron nitride nanosheet / aramid nanofiber composite thermally conductive film.
[0013] Preferably, in S1, the mass ratio of hexagonal boron nitride to sodium carboxymethyl cellulose is 1:(2-6), and the mass ratio of hexagonal boron nitride to hydroxyethyl cellulose is 1:(2-6).
[0014] Preferably, in S1: adding hexagonal boron nitride to a sodium carboxymethyl cellulose aqueous solution, followed by stirring for 40 to 50 hours to obtain a first suspension; adding hexagonal boron nitride to a hydroxyethyl cellulose aqueous solution, followed by stirring for 40 to 50 hours to obtain a second suspension.
[0015] Preferably, S2 is carried out according to the following process to obtain the first dispersion and the second dispersion respectively:
[0016] The homogenized first suspension is centrifuged at 7000-9000 rpm, the supernatant is removed and then washed with deionized water for 1-2 times to obtain a first dispersion;
[0017] The homogenized second suspension was first centrifuged at 7000-9000 rpm, and then the supernatant was removed and washed with deionized water for 1-2 times to obtain a second dispersion.
[0018] Further, S2 adopts the same deionized water washing process to obtain the first dispersion and the second dispersion, and the deionized water washing process is as follows:
[0019] Each time washing, deionized water was added first, then centrifuged at 3000-4000 rpm for 10-20 min, and the supernatant was discarded.
[0020] Preferably, the aramid nanofiber dispersion described in S3 is obtained by the following process:
[0021] The para-aramid fiber and KOH were dispersed in DMSO at a ratio of 1 g:1.5 g:500 mL to obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0022] Furthermore, in S3, the mass ratio of the boron nitride nanosheets in the first dispersion to the aramid nanofibers in the corresponding aramid nanofiber dispersion is 4:1, and the mass ratio of the boron nitride nanosheets in the second dispersion to the aramid nanofibers in the corresponding aramid nanofiber dispersion is 4:1.
[0023] Preferably, the film forming process described in S3 is vacuum filtration and hot pressing in sequence.
[0024] Furthermore, the hot pressing is performed at 210-230° C. for 8-12 minutes.
[0025] A boron nitride nanosheet / aramid nanofiber composite thermally conductive film obtained by the preparation method of the boron nitride nanosheet / aramid nanofiber composite thermally conductive film assisted by polymer exfoliation described in any one of the above.
[0026] Compared with the prior art, the present invention has the following beneficial technical effects:
[0027] The invention discloses a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, wherein h-BN is dispersed in a CMC aqueous solution and a HEC aqueous solution, and the concentration of the two polymer aqueous solutions is adjusted to thereby adjust the coating degree of the solution on the h-BN, thereby avoiding the polymerization of the h-BN, and relying on the impact on the inner wall of the homogeneous channel and the shear force during the exfoliation process, a BNNS with a high aspect ratio and low defects is prepared, thereby improving the intrinsic thermal conductivity of the BNNS. The more viscous the solution, the larger the coating surface of the h-BN is, and the more it can protect the h-BN from impact, and the less conducive it is to exfoliate the h-BN and obtain the BNNS with a high aspect ratio, and to maintain the lateral size of the BNNS, so the mass ratio of the two to deionized water is adjusted to a maximum of 1.5% to balance the interaction between the coating and the exfoliation at a high shear rate, and the coating effect is poor when the mass ratio is lower than 0.5%, and the h-BN is easily polymerized. The present invention makes full use of the water-soluble and thickening properties of CMC and HEC to increase the viscosity of the solution. The aqueous solution also has good dispersibility, which can effectively increase the dispersibility and stability of the two polymer particles in water, and ensure the good dispersion of h-BN during the homogenization process and the flow of the system during the homogenization process. CMC has a high thickening property, can provide a more suitable viscosity at a lower concentration, and shows good stability at a high shear rate, which is conducive to maintaining the uniformity and stability of the system; HEC has a relatively low thickening property, can provide a more suitable viscosity at a high shear rate, and HEC, as a non-ionic polymer, is not charged, which makes it highly compatible and will not cause adverse reactions. The present invention uses aramid nanofiber (ANF) as a polymer substrate and BNNS as a thermal conductive filler, peels off h-BN as much as possible without damaging the lateral size, and obtains boron nitride nanosheets with large size and small thickness, thereby improving the intrinsic thermal conductivity of BNNS. During the filling process, a boron nitride thermal conductive channel is built, and the establishment of the thermal conductive channel is conducive to phonon transfer, so that heat is rapidly diffused, and finally the thermal conductivity of the boron nitride nanosheet / aramid nanofiber composite film is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a SEM image of BNNS homogenized at 75 MPa with the assistance of HEC aqueous solution in Example 1 of the present invention.
[0029] Figure 2 2 are XRD patterns of the two BNNSs in Examples 3 and 6 of the present invention.
[0030] Figure 3 Graphs showing the thermal conductivity of two BNNS / ANF composite films in Examples 1 to 3 of the present invention.
[0031] Figure 4 Graphs showing the thermal conductivity of two BNNS / ANF composite films in Examples 4 to 6 of the present invention. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0033] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0034] Step (1), adding sodium carboxymethyl cellulose to three portions of 75 g of deionized water, wherein the ratio of sodium carboxymethyl cellulose to deionized water is 0.5%, 1% and 1.5%, respectively, and stirring for 2 hours to obtain three portions of completely dissolved CMC aqueous solutions for standby use;
[0035] Add hydroxyethyl cellulose to three portions of 75 g of deionized water, wherein the ratio of hydroxyethyl cellulose to deionized water is 0.5%, 1% and 1.5% respectively, and stir for 2 hours to obtain three portions of completely dissolved HEC aqueous solutions for later use;
[0036] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0037] Step (3), weigh 0.5 g of hexagonal boron nitride (h-BN), divide it into two equal parts, add them into a CMC aqueous solution and a HEC aqueous solution of the same specification prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain suspension a1 and suspension a2.
[0038] Step (4), taking the suspension a1 and the suspension a2 prepared in step (3), respectively homogenizing them by a micro-jet high-pressure homogenizer at a pressure of 75 to 90 MPa to achieve a peeling process, and preparing BNNS suspension a1 and BNNS suspension a2.
[0039] Step (5), taking the BNNS suspension a1 and the BNNS suspension a2 prepared in step (4), respectively, centrifuging them at 7000-9000 rpm, and then centrifuging and washing them with deionized water for 1-2 times to remove the polymers CMC and HEC, respectively. The deionized water centrifugal washing is specifically centrifuged at 3000-4000 rpm for 10-20 min, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0040] Step (6), take the two BNNS dispersions prepared in (5), mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (2), wherein the BNNS is 48 mg, vacuum filter them in turn, and hot press them at 220°C for 10 min to finally obtain two BNNS / ANF composite films.
[0041] Example 1
[0042] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0043] Step (1), weigh 1.125 g of CMC and HEC solid particles respectively, dissolve each in 75 g of water, and stir for 2 h to obtain CMC aqueous solution and HEC aqueous solution.
[0044] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0045] Step (3), weigh 0.5 g of h-BN, divide it into two equal parts, add them to the CMC aqueous solution and HEC aqueous solution prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain h-BN / CMC aqueous suspension and h-BN / HEC aqueous suspension.
[0046] Step (4), taking the h-BN / CMC aqueous suspension and the h-BN / HEC aqueous suspension prepared in step (3), respectively homogenizing them by a microjet high-pressure homogenizer at 75 MPa to achieve a stripping process to prepare a BNNS suspension.
[0047] Step (5), taking the BNNS suspension prepared in step (4), centrifuging at 8000 rpm, and then washing twice with deionized water to remove the polymers CMC and HEC. The deionized water centrifugal washing is specifically centrifuged at 3500 rpm for 15 minutes, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0048] Step (6), take the two portions of BNNS dispersion prepared in step (5), respectively mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (5), wherein each portion of BNNS is 48 mg, perform vacuum filtration in sequence, and hot press at 220° C. for 10 min, and finally obtain two portions of BNNS / ANF composite films.
[0049] Example 2
[0050] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0051] Step (1), weigh 0.75 g of CMC and HEC solid particles respectively, dissolve each in 75 g of water, and stir for 2 h to obtain CMC aqueous solution and HEC aqueous solution.
[0052] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0053] Step (3), weigh 0.5 g of h-BN, divide it into two equal parts, add them to the CMC aqueous solution and HEC aqueous solution prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain h-BN / CMC aqueous suspension and h-BN / HEC aqueous suspension.
[0054] Step (4), taking the h-BN / CMC aqueous suspension and the h-BN / HEC aqueous suspension prepared in step (3), respectively homogenizing them by a microjet high-pressure homogenizer at 75 MPa to achieve a stripping process to prepare a BNNS suspension.
[0055] Step (5), taking the BNNS suspension prepared in step (4), centrifuging at 8000 rpm, and then washing twice with deionized water to remove the polymers CMC and HEC. The deionized water centrifugal washing is specifically centrifuged at 3500 rpm for 15 minutes, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0056] Step (6), take the two portions of BNNS dispersion prepared in step (5), respectively mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (5), wherein each portion of BNNS is 48 mg, perform vacuum filtration in sequence, and hot press at 220° C. for 10 min, and finally obtain two portions of BNNS / ANF composite films.
[0057] Example 3
[0058] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0059] Step (1), weigh 0.375 g of CMC and HEC solid particles respectively, dissolve each in 75 g of water, and stir for 2 h to obtain CMC aqueous solution and HEC aqueous solution.
[0060] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0061] Step (3), weigh 0.5 g of h-BN, divide it into two equal parts, add them to the CMC aqueous solution and HEC aqueous solution prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain h-BN / CMC aqueous suspension and h-BN / HEC aqueous suspension.
[0062] Step (4), taking the h-BN / CMC aqueous suspension and the h-BN / HEC aqueous suspension prepared in step (3), respectively homogenizing them by a microjet high-pressure homogenizer at 75 MPa to achieve a stripping process to prepare a BNNS suspension.
[0063] Step (5), taking the BNNS suspension prepared in step (4), centrifuging at 8000 rpm, and then washing twice with deionized water to remove the polymers CMC and HEC. The deionized water centrifugal washing is specifically centrifuged at 3500 rpm for 15 minutes, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0064] Step (6), take the two portions of BNNS dispersion prepared in step (5), respectively mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (5), wherein each portion of BNNS is 48 mg, perform vacuum filtration in sequence, and hot press at 220° C. for 10 min, and finally obtain two portions of BNNS / ANF composite films.
[0065] Example 4
[0066] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0067] Step (1), weigh 1.125 g of CMC and HEC solid particles respectively, dissolve each in 75 g of water, and stir for 2 h to obtain CMC aqueous solution and HEC aqueous solution.
[0068] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0069] Step (3), weigh 0.5 g of h-BN, divide it into two equal parts, add them to the CMC aqueous solution and HEC aqueous solution prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain h-BN / CMC aqueous suspension and h-BN / HEC aqueous suspension.
[0070] Step (4), taking the h-BN / CMC aqueous suspension and the h-BN / HEC aqueous suspension prepared in step (3), respectively homogenizing them by a microjet high-pressure homogenizer at 90 MPa to achieve a stripping process to prepare a BNNS suspension.
[0071] Step (5), taking the BNNS suspension prepared in step (4), centrifuging at 8000 rpm, and then washing twice with deionized water to remove the polymers CMC and HEC. The deionized water centrifugal washing is specifically centrifuged at 3500 rpm for 15 minutes, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0072] Step (6), take the two portions of BNNS dispersion prepared in step (5), respectively mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (5), wherein each portion of BNNS is 48 mg, perform vacuum filtration in sequence, and hot press at 220° C. for 10 min, and finally obtain two portions of BNNS / ANF composite films.
[0073] Example 5
[0074] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0075] Step (1), weigh 0.75 g of CMC and HEC solid particles respectively, dissolve each in 75 g of water, and stir for 2 h to obtain CMC aqueous solution and HEC aqueous solution.
[0076] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0077] Step (3), weigh 0.5 g of h-BN, divide it into two equal parts, add them to the CMC aqueous solution and HEC aqueous solution prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain h-BN / CMC aqueous suspension and h-BN / HEC aqueous suspension.
[0078] Step (4), taking the h-BN / CMC aqueous suspension and the h-BN / HEC aqueous suspension prepared in step (3), respectively homogenizing them by a microjet high-pressure homogenizer at 90 MPa to achieve a stripping process to prepare a BNNS suspension.
[0079] Step (5), taking the BNNS suspension prepared in step (4), centrifuging at 8000 rpm, and then washing twice with deionized water to remove the polymers CMC and HEC. The deionized water centrifugal washing is specifically centrifuged at 3500 rpm for 15 minutes, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0080] Step (6), take the two portions of BNNS dispersion prepared in step (5), respectively mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (5), wherein each portion of BNNS is 48 mg, perform vacuum filtration in sequence, and hot press at 220° C. for 10 min, and finally obtain two portions of BNNS / ANF composite films.
[0081] Example 6
[0082] The present invention provides a method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, and the specific steps are as follows:
[0083] Step (1), weigh 0.375 g of CMC and HEC solid particles respectively, dissolve each in 75 g of water, and stir for 2 h to obtain CMC aqueous solution and HEC aqueous solution.
[0084] Step (2), weigh 1 g of para-aramid fiber and 1.5 g of KOH, disperse them in 500 mL of DMSO, and obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
[0085] Step (3), weigh 0.5 g of h-BN, divide it into two equal parts, add them to the CMC aqueous solution and HEC aqueous solution prepared in step (1), respectively, stir for 48 hours to fully mix, and obtain h-BN / CMC aqueous suspension and h-BN / HEC aqueous suspension.
[0086] Step (4), taking the h-BN / CMC aqueous suspension and the h-BN / HEC aqueous suspension prepared in step (3), respectively homogenizing them by a microjet high-pressure homogenizer at 90 MPa to achieve a stripping process to prepare a BNNS suspension.
[0087] Step (5), taking the BNNS suspension prepared in step (4), centrifuging at 8000 rpm, and then washing twice with deionized water to remove the polymers CMC and HEC. The deionized water centrifugal washing is specifically centrifuged at 3500 rpm for 15 minutes, pouring off the supernatant, retaining the precipitate, and obtaining two BNNS dispersions.
[0088] Step (6), take the two portions of BNNS dispersion prepared in step (5), respectively mix them evenly with 6 mL of the aramid nanofiber dispersion prepared in step (5), wherein each portion of BNNS is 48 mg, perform vacuum filtration in sequence, and hot press at 220° C. for 10 min, and finally obtain two portions of BNNS / ANF composite films.
[0089] from Figure 1 It can be seen that by adding polymer to assist exfoliation, h-BN can be exfoliated into BNNS with larger lateral dimensions. Therefore, homogenization can obtain BNNS with larger aspect ratio.
[0090] from Figure 2 It can be seen that the XRD peaks of all BNNS powder samples detected are shifted compared with the peak of standard h-BN (26.8°), indicating that this method can indeed peel off the h-BN and shear it into thin sheets.
[0091] from Figure 3It can be seen that under a pressure of 75 MPa, as the polymer concentration decreases, the thermal conductivity of the prepared film increases, indicating that reducing the concentrations of CMC and BNNS can increase the aspect ratio of BNNS during the homogenization process, thereby increasing the thermal conductivity of the film after assembly.
[0092] from Figure 4 It can be seen that under a pressure of 90 MPa, as the concentration of HEC solution decreases, the thermal conductivity of the prepared film increases, and under the same conditions, the thermal conductivity of the film is lower than that under a pressure of 75 MPa, indicating that the BNNS prepared at 75 MPa has a relatively better effect; and as the concentration of CMC solution decreases, the thermal conductivity of the prepared film decreases. This is because under a pressure of 90 MPa, CMC and BNNS have obvious electrostatic effects, and CMC is modified on BNNS. Thermogravimetric detection shows that the higher the CMC concentration, the higher the modification amount. Since new functional groups are introduced on BNNS, the higher the modification amount, the more conducive to the improvement of the thermal conductivity of the film.
Claims
1. A method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film, characterized in that: The steps include: S1, dispersing hexagonal boron nitride into a sodium carboxymethyl cellulose aqueous solution, wherein the mass ratio of sodium carboxymethyl cellulose to deionized water in the sodium carboxymethyl cellulose aqueous solution is (0.5-1.5):100, to obtain a first suspension; Dispersing hexagonal boron nitride in a hydroxyethyl cellulose aqueous solution, wherein the mass ratio of hydroxyethyl cellulose to deionized water in the hydroxyethyl cellulose aqueous solution is (0.5-1.5):100, to obtain a second suspension; S2, homogenizing the first suspension at 75-90 MPa, and then separating the sodium carboxymethyl cellulose therein to obtain a first dispersion; homogenizing the second suspension at 75-90 MPa, and then separating the hydroxyethyl cellulose therein to obtain a second dispersion; S3, respectively mixing the first dispersion and the second dispersion with the aramid nanofiber dispersion, and then performing a film forming process to obtain a boron nitride nanosheet / aramid nanofiber composite thermal conductive film.
2. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 1, characterized in that: In S1, the mass ratio of hexagonal boron nitride to sodium carboxymethyl cellulose is 1:(2-6), and the mass ratio of hexagonal boron nitride to hydroxyethyl cellulose is 1:(2-6).
3. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 1, characterized in that: In S1: adding hexagonal boron nitride to a sodium carboxymethyl cellulose aqueous solution, followed by stirring for 40 to 50 hours to obtain a first suspension; adding hexagonal boron nitride to a hydroxyethyl cellulose aqueous solution, followed by stirring for 40 to 50 hours to obtain a second suspension.
4. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 1, characterized in that: S2 is carried out as follows to obtain the first dispersion and the second dispersion respectively: The homogenized first suspension is centrifuged at 7000-9000 rpm, the supernatant is removed and then washed with deionized water for 1-2 times to obtain a first dispersion; The homogenized second suspension was first centrifuged at 7000-9000 rpm, and then the supernatant was removed and washed with deionized water for 1-2 times to obtain a second dispersion.
5. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 4, characterized in that: S2 uses the same deionized water washing process to obtain the first dispersion and the second dispersion, and the deionized water washing process is as follows: Each time washing, deionized water was added first, then centrifuged at 3000-4000 rpm for 10-20 min, and the supernatant was discarded.
6. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 1, characterized in that: The aramid nanofiber dispersion described in S3 is obtained by the following process: The para-aramid fiber and KOH were dispersed in DMSO at a ratio of 1 g:1.5 g:500 mL to obtain an aramid nanofiber dispersion with a concentration of 2 mg / mL.
7. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 6, characterized in that: In S3, the mass ratio of boron nitride nanosheets in the first dispersion to aramid nanofibers in the corresponding aramid nanofiber dispersion is 4:1, and the mass ratio of boron nitride nanosheets in the second dispersion to aramid nanofibers in the corresponding aramid nanofiber dispersion is 4:
1.
8. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 1, characterized in that: The film forming processes described in S3 are vacuum filtration and hot pressing.
9. The method for preparing the polymer-assisted exfoliation boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to claim 8, characterized in that: The hot pressing is carried out at 210-230° C. for 8-12 minutes.
10. A boron nitride nanosheet / aramid nanofiber composite thermally conductive film obtained by the method for preparing a polymer-assisted exfoliated boron nitride nanosheet / aramid nanofiber composite thermally conductive film according to any one of claims 1 to 9.
Citation Information
Patent Citations
Boron nitride heat dissipation film and preparation method and application thereof
CN113179611A
Boron nitride nanosheet / aramid nanofiber composite film prepared by ball-milling hydroxyethyl cellulose and preparation method of boron nitride nanosheet / aramid nanofiber composite film
CN117304535A
Coating for high-performance abrasive paper and preparation method thereof
CN118185448A
Boron nitride heat dissipation film, preparation method therefor, and application thereof
WO2022193572A1
Cited By
Waterproof agent emulsion as well as preparation method and application thereof