X-ray response film, preparation method and application thereof

By preparing X-ray-responsive films doped with copper complexes and organic hydrazone compounds on a flexible substrate, the problem of inconspicuous response and irreversible signal in existing materials under low dose X-rays is solved, and the production under low dose X-rays is achieved The effect of obvious optical signals and recyclable use is suitable for medical and industrial testing.

CN118909289APending Publication Date: 2024-11-08NANJING UNIV OF POSTS & TELECOMM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135540.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing X-ray-responsive materials respond insignificantly under low dose X-rays and the optical signal is irreversible, limiting their application value in medical imaging and industrial detection.

Method used

X-ray response film was prepared on a flexible substrate using copper complex Cu2I2(POP)2 and organic hydrazone compounds (Hzld-H, Hzld-Br, Hzld-I) and polyacrylamide, and physical doping and ultrasonic uniformity through specific proportions. The mixture was processed and then applied driply and heated to dry, resulting in a film capable of producing significant optical signal transitions under low dose X-rays and recoverable by heat treatment.

Benefits of technology

This X-ray-responsive film produces obvious optical signal transformation under extremely low X-ray radiation dose. It has strong real-time performance, simple operation, and can recover optical properties after heat treatment. It is suitable for medical imaging and industrial detection, reducing the use of products cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909289A_ABST
    Figure CN118909289A_ABST
Patent Text Reader

Abstract

The invention discloses an X-ray response film as well as a preparation method and application thereof, and belongs to the technical field of photoluminescent materials. The preparation method comprises the following steps: physically doping the copper complex (Cu2I2 (POP) 2) and the organic hydrazone compounds (Hz1d-H, Hz1d-Br and Hz1d-I) into polyacrylamide (PMMA) according to a specific ratio to prepare a mixed solution, dispensing the mixed solution onto a flexible substrate, and heating and drying to obtain the flexible copper complex / organic hydrazone composite material. The obtained product has good response capability to X-rays, can generate very obvious optical signal conversion under extremely low X-ray radiation dose (mGy level), and has the advantages of strong real-time performance, simplicity in operation and the like, and the optical property of the film can be recovered again after heat treatment, so that the film has good recycling capability; the film has wide application prospects in the fields of medical imaging and industrial detection, and is expected to be further developed into a full-digital imaging solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photoluminescent materials, and in particular relates to an X-ray responsive film, a preparation method and applications thereof in X-ray imaging and industrial flaw detection. Background Art

[0002] Since 1895, X-rays have become an indispensable tool in many fields, including medical diagnosis and industrial inspection. Early X-ray imaging mainly relied on X-ray film, which used chemical reactions caused by X-ray exposure to produce images. However, film imaging required tedious and time-consuming wet processing, which affected its further development.

[0003] In recent years, digital radiography (DR) and computed radiography (CR) have gradually replaced traditional X-ray films in many application scenarios due to their convenient imaging characteristics. However, this type of imaging technology is not without disadvantages. High cost and low equipment feasibility are the main reasons limiting the popularization of such technology. Therefore, film-based imaging technology still plays an important role in some resource-constrained environments and certain industrial application scenarios.

[0004] In order to break the limitations of traditional X-ray imaging technology, it is of great significance to develop new X-ray responsive materials. Existing reported new X-ray responsive materials will produce substantial changes in optical properties when exposed to X-rays, without the need for traditional darkroom processing, greatly simplifying the imaging procedure. In addition, the resulting light signal changes can be directly captured by light sensors or high-resolution cameras, facilitating digital storage and remote transmission. This improvement can not only promote the rapid development of modern medical imaging, but also meet the needs of industrial automation. Compared with traditional X-ray films, X-ray responsive imaging technology has the advantages of strong real-time performance and simple operation, and has broad application prospects in the future fields of medical imaging and industrial detection.

[0005] However, one thing that still needs to be considered is that most of the existing X-ray responsive materials require high radiation doses to produce optical signal changes and most of these changes are irreversible, that is, the optical signals generated by the materials are not cyclical and cannot be recycled, which will undoubtedly affect the practical application value of such materials. Therefore, the development of new high-sensitivity X-ray responsive materials that can quickly and reliably switch optical signals when exposed to low-dose X-rays is crucial to promoting technological advances in medical imaging and industrial detection. Summary of the invention

[0006] In order to solve the deficiencies in the prior art, the present invention provides an X-ray responsive film which can quickly and reliably switch optical signals when exposed to low-dose X-rays, and discloses a specific preparation method thereof.

[0007] In order to achieve the above technical objectives, the present invention is implemented by the following technical scheme: A method for preparing an X-ray responsive film comprises the following steps:

[0008] 1) dissolving polyacrylamide in an organic solvent to obtain solution A;

[0009] 2) dissolving a hydrazone compound having the following structure in an organic solvent to obtain solution B;

[0010]

[0011] Wherein, X=H, Br or I;

[0012] 3) Mix the copper complex Cu2I2(POP)2 with the following structure and an organic solvent, mix by ultrasonication, and add solution B and solution A to mix;

[0013]

[0014] 4) Spread the mixed solution prepared in the previous step on a flexible substrate, evaporate it at room temperature overnight, and dry it on a heating platform to obtain an X-ray responsive film.

[0015] Furthermore, in step 1), the organic solvent used is chloroform, and the concentration of polyacrylamide in solution A is 10-200 mg / mL.

[0016] Furthermore, in step 2), the organic solvent used is chloroform, and the concentration of the hydrazone compound in solution B is 0.001-0.01 mg / μL.

[0017] Furthermore, in step 3), the organic solvent used is chloroform, the mass ratio of the hydrazone compound to the copper complex in the mixed solution is 0.005-0.07:1, and the mass ratio of the copper complex to polyacrylamide is 1:10.

[0018] Furthermore, in step 4), the temperature of the heating platform is 40-50° C., and the heating and drying time is 6-8 hours.

[0019] The X-ray responsive film prepared based on the above preparation method can be used as a core component in X-ray responsive imaging technology or radiation detectors. The X-ray responsive film can produce obvious optical signal transformation under an X-ray radiation dose of 100 to 400 mGy, and the optical properties of the film can be restored again after heat treatment.

[0020] Furthermore, the heat treatment temperature is 60-80°C.

[0021] The above-mentioned X-ray responsive film can be used in medical imaging, industrial inspection and other fields, and is expected to be further developed into a fully digital imaging solution.

[0022] The beneficial effects of the present invention are:

[0023] 1. The X-ray responsive film disclosed in the present application is prepared by physically doping a copper complex (Cu2I2(POP)2) and an organic hydrazone compound (Hzld-H, Hzld-Br, Hzld-I) in a specific ratio into polyacrylamide (PMMA) to prepare a mixed solution, which is then drop-coated onto a flexible PET substrate. The obtained product has good response to X-rays and can produce a very obvious optical signal change at an extremely low X-ray radiation dose (mGy level). It has the advantages of strong real-time performance and simple operation, and can be used as a core component of a recording radiation imaging film or a radiation detector, and has broad application prospects in many fields such as security inspection, medical imaging, and quality inspection.

[0024] 2. The X-ray responsive film disclosed in the present application not only has good X-ray responsiveness, but also the optical properties of the film that undergoes optical signal transformation under X-ray radiation can be restored after heat treatment, so that the film can be recycled, reducing the use cost of the product;

[0025] 3. The preparation method of the X-ray responsive film disclosed in the present application is simple, the raw materials used are cheap and easy to obtain, and the product has the advantages of low toxicity, low cost, and can be produced on a flexible substrate, all of which facilitate the large-scale preparation of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 These are the XRD simulation data and test data of Cu2I2(POP)2 prepared in Example 1;

[0027] Figure 2 Panels a, b, and c are respectively the mass spectra of Hzld-H, Hzld-Br, and Hzld-I prepared in Example 1;

[0028] Figure 3A is the NMR image of Hzld-H prepared in Example 1;

[0029] Figure 3B is the NMR image of Hzld-Br prepared in Example 1;

[0030] Figure 3C is the NMR image of Hzld-1 prepared in Example 1;

[0031] Figure 4 This is a photograph of the X-ray responsive film Cu2I2(POP)2 / Hzld-I prepared in Example 1;

[0032] Figure 5Panels a, b, and c are respectively the excitation-emission spectra of Cu2I2(POP)2 / Hzld-H, Cu2I2(POP)2 / Hzld-Br and Cu2I2(POP)2 / Hzld-I films prepared in Example 1 after irradiation with different X-ray doses;

[0033] Figure 6 Small figures a, b and c are emission spectra of the Cu2I2(POP)2 / Hzld-H, Cu2I2(POP)2 / Hzld-Br and Cu2I2(POP)2 / Hzld-I films prepared in Example 1 after being irradiated during the heat treatment process;

[0034] Figure 7 is a schematic diagram of the response mechanism of the X-ray responsive film prepared in Example 1;

[0035] Figure 8 It is the emission intensity cycle diagram of the X-ray responsive film prepared in Example 1 under the cyclic action of X-ray radiation and heat treatment, wherein, sub-diagram a is the emission intensity cycle diagram of Cu2I2(POP)2 / Hzld-H, sub-diagram b is the emission intensity cycle diagram of Cu2I2(POP)2 / Hzld-Br, and sub-diagram c is the emission intensity cycle diagram of Cu2I2(POP)2 / Hzld-I;

[0036] Fig. 9 This is an imaging application diagram of the X-ray responsive film Cu2I2(POP)2 / Hzld-I prepared in Example 1. DETAILED DESCRIPTION

[0037] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.

[0038] Example 1

[0039] Step 1, preparation of copper complex (Cu2I2(POP)2)

[0040] The preparation route is as follows:

[0041]

[0042] The specific preparation process is as follows: di(2-diphenylphosphinophenyl) ether and cuprous iodide are taken in a molar ratio of 1:1, acetonitrile solvent is added to dissolve, and then the reaction system is heated to 180°C in a reactor and reacted for 48 hours, and then the heating device is turned off and allowed to stand for 24 hours to obtain a copper complex Cu2I2(POP)2 of di(2-diphenylphosphinophenyl) ether and cuprous iodide. Figure 1These are the XRD simulation data and test data of Cu2I2(POP)2.

[0043] Step 2, preparation of organic hydrazone compounds (Hzld-H, Hzld-Br, Hzld-I)

[0044] The general formula of organic hydrazone compounds is as follows:

[0045]

[0046] Wherein, X=H, Br or I; when X is H, the compound is recorded as Hzld-H; when X is Br, the compound is recorded as Hzld-Br; when X is I, the compound is recorded as Hzld-I.

[0047] The synthetic route is as follows:

[0048]

[0049] The specific preparation process is:

[0050] 1) Dissolve 4-bromo-N,N-dimethylaniline (3g) in anhydrous tetrahydrofuran. At -78°C, add n-butyl lithium (1.6M, 9.46mL) dropwise and react for 15min, then add diethyl oxalate (3.26mL); react the mixture at -78°C for half an hour. Slowly restore the room temperature and then add water to quench the reaction; extract with water / dichloromethane and collect the organic layer. After removing the organic solvent, purify the organic layer by column chromatography, and purify with petroleum ether and dichloromethane (1:5, v / v) as eluents to obtain a bright yellow solid compound, namely compound 1;

[0051] 2) Phenylhydrazine-X (390 mg when X = H, 335 mg when X = Br, 295 mg when X = I) and acetic acid (HOAc, 0.2 mL) were added to an ethanol solution of compound 1 (500 mg). The resulting mixture was heated to 80 ° C in a nitrogen atmosphere and refluxed overnight. After the reaction was completed, ethanol was removed and the resulting crude residue was dissolved in dichloromethane, washed with a saturated sodium bicarbonate solution, and then dried over anhydrous sodium sulfate. After removing the organic solvent, column chromatography was used for purification using petroleum ether / dichloromethane (6:1, v / v) as an eluent to obtain hydrazone compounds Hzld-H, Hzld-Br and Hzld-I.

[0052] Step 3: Preparation of X-ray responsive film

[0053] 1) Take 2g polyacrylamide (PMMA) and 20mL chloroform and add them to a glass bottle, add a magnetic stirrer until completely dissolved, and obtain solution A (PMMA concentration 100mg / mL); take 2mg of the hydrazone compound (any one of Hzld-H, Hzld-Br and Hzld-I) prepared in step 2 and dissolve it in 2mL chloroform to prepare solution B (hydrazone compound concentration 0.001mg / μL);

[0054] 2) Add 10 mg Cu2I2(POP)2 and 500 μL chloroform to a 3 mL glass bottle and mix them evenly by ultrasonication; then add 500 μL prepared solution B and 1 mL solution A, add a magnetic stirrer for 4 h to obtain a mixed solution;

[0055] 3) Take 1 mL of the mixed solution prepared in step 2) and drop it on a clean PET film (3 cm × 4 cm, 0.075 mm thick), slowly evaporate it at room temperature overnight, and then continue to dry it on a heating table at 40°C for 8 h to obtain an X-ray responsive film. Based on the different selected hydrazone compounds, the three X-ray responsive films obtained were respectively recorded as Cu2I2(POP)2 / Hzld-H, Cu2I2(POP)2 / Hzld-Br and Cu2I2(POP)2 / Hzld-I.

[0056] The photo of the prepared X-ray responsive film Cu2I2(POP)2 / Hzld-I is shown in Figure 4 shown.

[0057] Response behavior test:

[0058] The excitation-emission spectra of the Cu2I2(POP)2 / Hzld-H, Cu2I2(POP)2 / Hzld-Br and Cu2I2(POP)2 / Hzld-I X-ray response films prepared in this embodiment after irradiation with different X-ray doses were measured using an Edinburgh F980 transient spectrometer, as shown in FIG. Figure 5 As shown in the a, b, and c panels, the emission peaks of the three X-ray films are at 514nm, 516nm, and 516nm, respectively. In the test of X-ray response, it was observed that the emission intensity of Cu2I2(POP)2 / Hzld-H film decreased by 2.7 times after absorbing 335.80mGy of X-rays; the emission intensity of Cu2I2(POP)2 / Hzld-Br film decreased by 3.6 times after absorbing 244.21mGy of X-rays; and the emission intensity of Cu2I2(POP)2 / Hzld-I film decreased by 5.5 times after absorbing 213.68mGy of X-rays. All three films have sensitive response behavior to X-rays, and their optical signals can change significantly at low radiation doses (radiation doses of the order of mGy).

[0059] The study found that the change in optical signal is caused by Cu2I2(POP)2 converting X-ray energy to sensitize the triplet state of the organic hydrazone compound, resulting in a ZE configuration change of the hydrazone compound, such as Figure 7 As shown in the figure, after Cu2I2(POP)2 absorbs X-rays, it generates high-energy electrons, which are injected into the singlet and triplet emission energy levels of Cu2I2(POP)2 at a ratio of 1:3. Then the energy is transferred from the triplet state of Cu2I2(POP)2 to the triplet state (TTET) of the hydrazone compound. Finally, the energy causes the hydrazone compound to transform from the luminescent state Z configuration to the non-luminescent state E configuration in the form of non-radiative transition.

[0060] The irradiated X-ray response film was placed in an environment of 70°C. During the slow heating process of the irradiated X-ray response film, it was found that the emission intensity of the film gradually recovered, such as Figure 6 This is because the hydrazone structure changes from E to Z during the heat treatment process, as shown in Figure 7 As shown. Under the cyclic action of X-ray irradiation and heat treatment, the optical signal of the prepared X-ray response film has good cyclic properties, such as Figure 8 shown.

[0061] Application Example 1

[0062] The X-ray responsive film Cu2I2(POP)2 / Hzld-I was prepared according to the method in Example 1. Since different materials in the imaging object have different absorption capabilities for X-rays, the transmitted X-rays have different attenuation degrees. Therefore, after being exposed to different doses of X-rays, the responsive film will show the appearance of the internal structure of the imaging object. Fig. 9 As shown, the Cu2I2(POP)2 / Hzld-I film recorded the detailed structure inside the chip. It showed its good imaging effect and resolution as an X-ray film. The X-ray responsive film prepared by the present invention has the advantages of low toxicity, low cost, and can be mass-produced on a flexible substrate.

[0063] Example 2

[0064] Step 1 and step 2 of this embodiment are the same as those in Example 1, that is, the copper complex (Cu2I2(POP)2) and organic hydrazone compound (Hzld-H, Hzld-Br, Hzld-I) used for preparing the X-ray responsive film are the same.

[0065] Step 3: Preparation of X-ray responsive film

[0066] 1) Same as Example 1;

[0067] 2) Add 10 mg Cu2I2(POP)2 and 600 μL chloroform to a 3 mL glass bottle and mix them evenly by ultrasonication; then add 400 μL prepared solution B and 1 mL solution A, add a magnetic stirrer for 4 h to obtain a mixed solution;

[0068] 3) Same as Example 1.

[0069] Example 3

[0070] Step 1: Same as Example 1.

[0071] Step 2: Same as Example 1.

[0072] Step 3: Preparation of X-ray responsive film

[0073] 1) Same as Example 1;

[0074] 2) Add 10 mg Cu2I2(POP)2 and 700 μL chloroform to a 3 mL glass bottle and mix them evenly by ultrasonication; then add 300 μL prepared solution B and 1 mL solution A, add a magnetic stirrer for 4 h to obtain a mixed solution;

[0075] 3) Same as Example 1.

[0076] Example 4

[0077] Step 1: Same as Example 1.

[0078] Step 2: Same as Example 1.

[0079] Step 3: Preparation of X-ray responsive film

[0080] 1) Same as Example 1;

[0081] 2) Add 10 mg Cu2I2(POP)2 and 800 μL chloroform to a 3 mL glass bottle and mix them evenly by ultrasonication; then add 200 μL prepared solution B and 1 mL solution A, add a magnetic stirrer for 4 h to obtain a mixed solution;

[0082] 3) Same as Example 1.

[0083] Example 5

[0084] Step 1: Same as Example 1.

[0085] Step 2: Same as Example 1.

[0086] Step 3: Preparation of X-ray responsive film

[0087] 1) Same as Example 1;

[0088] 2) Add 10 mg Cu2I2(POP)2 and 950 μL chloroform to a 3 mL glass bottle and mix them evenly with ultrasound; then add 50 μL of the prepared solution B and 1 mL of solution A, add a magnetic stirrer for 4 h to obtain a mixed solution;

[0089] 3) Same as Example 1.

[0090] Example 6

[0091] Step 1: Same as Example 1.

[0092] Step 2: Same as Example 1.

[0093] Step 3: Preparation of X-ray responsive film

[0094] 1) Same as Example 1;

[0095] 2) Add 10 mg Cu2I2(POP)2 and 300 μL chloroform to a 3 mL glass bottle and mix them evenly by ultrasonication; then add 700 μL prepared solution B and 1 mL solution A, add a magnetic stirrer for 4 h to obtain a mixed solution;

[0096] 3) Same as Example 1.

[0097] The difference between Examples 1-6 is that when preparing the X-ray responsive film, the volumes of chloroform and solution B used to prepare the mixed solution of Cu2I2(POP)2, solution A and solution B are different (see Table 1), but in order to maintain the uniformity of the coating, the total volume of the prepared solution is controlled to be uniformly 2 mL.

[0098] Table 1. Material ratios for preparing X-ray responsive films

[0099]

[0100]

[0101] Through experiments, it was found that as the proportion of hydrazone compounds (any one of Hzld-H, Hzld-Br and Hzld-I) in the mixed solution gradually increased, the responsiveness of the X-ray responsive film to X-rays showed a trend of first increasing and then decreasing. When the mass ratio of hydrazone compounds to Cu2I2(POP)2 was 0.05:1, the prepared X-ray responsive film had the best performance.

[0102] The above shows and describes the basic principles, main features and advantages of the present invention. However, the above is only a specific embodiment of the present invention, and the technical features of the present invention are not limited thereto. Any other implementation methods derived by any technician in the field without departing from the technical solution of the present invention should be included in the patent scope of the present invention.

Claims

1. A method for preparing an X-ray responsive film, characterized in that: The steps include: 1) dissolving polyacrylamide in an organic solvent to obtain solution A; 2) dissolving a hydrazone compound having the following structure in an organic solvent to obtain solution B; Wherein, X=H, Br or I; 3) Mix the copper complex Cu2I2(POP)2 with the following structure and an organic solvent, mix by ultrasonication, and add solution B and solution A to mix; 4) Spread the mixed solution prepared in the previous step on a flexible substrate, evaporate it at room temperature overnight, and dry it on a heating platform to obtain an X-ray responsive film.

2. The method for preparing an X-ray responsive film according to claim 1, characterized in that: In step 1), the organic solvent used is chloroform, and the concentration of polyacrylamide in solution A is 10-200 mg / mL.

3. The method for preparing an X-ray responsive film according to claim 1, characterized in that: In step 2), the organic solvent used is chloroform, and the concentration of the hydrazone compound in solution B is 0.001-0.01 mg / μL.

4. The method for preparing an X-ray responsive film according to claim 1, characterized in that: In step 3), the organic solvent used is chloroform, the mass ratio of the hydrazone compound to the copper complex in the mixed solution is 0.005-0.07:1, and the mass ratio of the copper complex to polyacrylamide is 1:

10.

5. The method for preparing an X-ray responsive film according to claim 1, characterized in that: In step 4), the temperature of the heating platform is 40-50° C., and the heating and drying time is 6-8 hours.

6. X-ray responsive film, characterized in that, It is prepared based on the preparation method described in any one of claims 1 to 5, and can be used as a core component in X-ray response imaging technology or radiation detectors.

7. The X-ray responsive film according to claim 6, characterized in that: The X-ray responsive film can produce an obvious optical signal conversion under an X-ray radiation dose of 100 to 400 mGy, and the optical properties of the film can be restored again after heat treatment.

8. The X-ray responsive film according to claim 7, characterized in that: The heat treatment temperature is 60-80°C.

9. Use of the X-ray responsive film as claimed in claim 8 in the field of medical imaging.

10. Application of the X-ray responsive film as claimed in claim 8 in the field of industrial detection.