High-temperature-resistant flame-retardant foam and preparation method thereof
By using base layer formulas of materials such as silicone rubber, vinyl silicone oil and other materials in foam and modifying technology of modified fillers, combined with conductive layer composite, the problem of foam is not resistant to high temperature and flame retardant, and higher resistance is achieved High temperature and flame retardant properties.
Patent Information
- Application Number
- CN202410952481.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional foams are not resistant to high temperatures and lack flame retardant properties, which limits their application in certain fields.
The base layer formula including silicone rubber, vinyl silicone oil, modified fillers, phenolic resin, crosslinking agent, foaming agent and catalyst are adopted, and the high temperature resistance of foam is improved through the preparation of modified fillers and the composite technology of conductive layers. Flame retardant performance.
It significantly improves the high temperature resistance and flame retardant properties of foam, making it stable in high temperature environments, and is suitable for a wider range of application scenarios.
Smart Images

Figure BDA0004947604530000071 
Figure BDA0004947604530000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of conductive foam, and in particular to a high temperature resistant flame retardant foam and a preparation method thereof. Background Art
[0002] Foam is a material made by foaming plastic particles, referred to as foam. Foam is widely used in the fields of electronic technology and military industry because of its elasticity, light weight, fast pressure-sensitive fixation, small size, and stable performance. Common foam materials include polyethylene foam, polyester foam, rubber foam, etc. Some materials combine foam with other materials through simple physical coating, while some are directly bonded to the corresponding material by practical foaming process on the surface of the corresponding material. However, conventional foam is not resistant to high temperature during use, and is prone to falling off and damage under high temperature conditions. It also does not have flame retardant properties, which affects its application in some fields. Summary of the invention
[0003] In order to improve the high temperature resistance and flame retardancy of foam, the present application provides a high temperature resistant and flame retardant foam and a preparation method thereof.
[0004] In the first aspect, the present application provides a high temperature resistant flame retardant foam, which adopts the following technical solution: A high-temperature resistant flame-retardant foam comprises a base layer and a conductive layer. The raw materials of the base layer comprise the following components in parts by weight: 20 to 30 parts of silicone rubber, 5 to 10 parts of vinyl silicone oil, 5 to 15 parts of modified fillers, 1 to 5 parts of phenolic resin, 10 to 15 parts of cross-linking agents, 5 to 10 parts of foaming agents, and 0.5 to 1 part of catalysts; the raw materials of the modified fillers comprise γ-aminopropyltriethoxysilane, an organic solvent, carbon nanotubes, and aluminum hydroxide.
[0005] By adopting the above technical scheme, γ-aminopropyltriethoxysilane is dissolved by an organic solvent, and then carbon nanotubes and aluminum hydroxide are modified to obtain a modified filler with good dispersion effect. The carbon nanotubes have good thermal conductivity, and aluminum hydroxide will decompose to produce water at high temperature, so that the base layer has good high temperature flame retardant properties; silicone rubber and phenolic resin have good high temperature flame retardant properties, and the cross-linking agent and γ-aminopropyltriethoxysilane on the surface of the modified filler are used to combine the two, thereby further improving the high temperature flame retardant properties of the final foam.
[0006] In a specific embodiment, the method for preparing the modified filler comprises the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified liquid; stir and mix carbon nanotubes and aluminum hydroxide evenly to obtain a mixture, then spray the modified liquid into the mixture while stirring the mixture, continue stirring after spraying, and dry to obtain a modified filler.
[0007] By adopting the above technical scheme, γ-aminopropyltriethoxysilane is first dissolved in an organic solvent to obtain a modified liquid, and then the modified liquid is sprayed while stirring carbon nanotubes and aluminum hydroxide. After spraying, the mixture is continued to be stirred and then dried to obtain a modified filler with good dispersibility.
[0008] In a specific embodiment, the weight ratio of the modified liquid to the mixed material is 1:(13-14).
[0009] By adopting the above technical solution, the ratio of the modified liquid to the mixed material is further limited, so that γ-aminopropyltriethoxysilane can better modify the carbon nanotubes and aluminum hydroxide, further improving the dispersion effect of the modified filler.
[0010] In a specific embodiment, the crosslinking agent includes hydrogen-containing silicone oil.
[0011] In a specific embodiment, the foaming agent includes a mixture of sodium ricinoleate and dimethicone.
[0012] By adopting the above technical solution, sodium ricinoleate has a good foaming effect, and dimethyl silicone oil can make the foaming stable and uniform, so the combination of the two improves the foaming effect of the final base layer.
[0013] In a specific embodiment, the catalyst comprises a platinum catalyst.
[0014] In a specific embodiment, the raw materials of the base layer further include 5 to 7 parts by weight of melamine polyphosphate.
[0015] By adopting the above technical solution, the addition of melamine polyphosphate can play an auxiliary flame retardant role and further improve the flame retardant properties of the final foam.
[0016] In a specific embodiment, the raw materials of the base layer further include 5 to 10 parts by weight of wollastonite powder and 5 to 10 parts by weight of talc powder.
[0017] By adopting the above technical solution, both wollastonite powder and talcum powder have good high temperature resistance, and talcum powder can also make the raw materials in the base layer evenly dispersed, thereby improving the performance of the high temperature resistant flame retardant foam.
[0018] In a specific embodiment, the conductive layer is a copper-plated layer and a gold-plated layer.
[0019] In a second aspect, the present application provides a method for preparing a high temperature resistant flame retardant foam, which adopts the following technical solution: A method for preparing a high temperature resistant flame retardant foam comprises the following steps: The silicone rubber, vinyl silicone oil, modified filler, phenolic resin, crosslinking agent, foaming agent, catalyst and other raw materials are stirred and mixed uniformly to obtain a coarse material; The coarse material is extruded and formed to obtain a silicone core; the formed silicone core is pulled into a dryer for drying; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam.
[0020] By adopting the above technical scheme, silicone rubber, vinyl silicone oil, modified filler, phenolic resin, crosslinking agent, foaming agent, catalyst and other raw materials are first mixed, then extruded and molded, dried, and finally compounded with a conductive layer and cut to obtain high temperature resistant flame retardant foam.
[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. In the present application, γ-aminopropyltriethoxysilane is dissolved by an organic solvent, and then carbon nanotubes and aluminum hydroxide are modified to obtain a modified filler with good dispersion effect. The carbon nanotubes have good thermal conductivity, and aluminum hydroxide decomposes to produce water at high temperature, so that the base layer has good high temperature flame retardant properties; silicone rubber and phenolic resin have good high temperature flame retardant properties, and the crosslinking agent and γ-aminopropyltriethoxysilane on the surface of the modified filler are used to combine the two, thereby further improving the high temperature flame retardant properties of the final foam; 2. In this application, both wollastonite powder and talcum powder have good high temperature resistance, and talcum powder can also make the raw materials in the base layer evenly dispersed, thereby improving the performance of high temperature resistant flame retardant foam; 3. The method of the present application first mixes silicone rubber, vinyl silicone oil, modified filler, phenolic resin, crosslinking agent, foaming agent, catalyst and other raw materials, then extrude and shape, dry, and finally compound the conductive layer and cut to obtain high temperature resistant flame retardant foam. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments.
[0023] All raw materials in the examples can be obtained from commercial sources, including phenolic resin CAS No.: 9003-35-4; platinum catalyst CAS No.: 68478-92-2.
[0024] Preparation Example Preparation Example 1 Preparation Example 1 provides a method for preparing a modified filler, comprising the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified liquid; wherein the weight ratio of the organic solvent, water and γ-aminopropyltriethoxysilane is 18:2:5; the organic solvent is ethanol; The carbon nanotubes and aluminum hydroxide are stirred and mixed evenly to obtain a mixture, and then the modifying liquid is slowly sprayed into the mixture while stirring the mixture. After the spraying is completed, the mixture is stirred for 0.5 hours, and then dried at 110 degrees Celsius for 1 hour to obtain a modified filler; wherein the weight ratio of the carbon nanotubes to the aluminum hydroxide is 1:2; the weight ratio of the modifying liquid to the mixture is 1:12.5.
[0025] Preparation Example 2 Preparation Example 2 provides a method for preparing a modified filler, comprising the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified liquid; wherein the weight ratio of the organic solvent, water and γ-aminopropyltriethoxysilane is 18:2:5; the organic solvent is ethanol; The carbon nanotubes and aluminum hydroxide are stirred and mixed evenly to obtain a mixture, and then the modifying liquid is slowly sprayed into the mixture while stirring the mixture. After the spraying is completed, the mixture is stirred for 0.5 hours, and then dried at 110 degrees Celsius for 1 hour to obtain a modified filler; wherein the weight ratio of the carbon nanotubes to the aluminum hydroxide is 1:2; the weight ratio of the modifying liquid to the mixture is 1:13.
[0026] Preparation Example 3 Preparation Example 3 provides a method for preparing a modified filler, comprising the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified liquid; wherein the weight ratio of the organic solvent, water and γ-aminopropyltriethoxysilane is 18:2:5; the organic solvent is ethanol; The carbon nanotubes and aluminum hydroxide are stirred and mixed evenly to obtain a mixture, and then the modifying liquid is slowly sprayed into the mixture while stirring the mixture. After the spraying is completed, the mixture is stirred for 0.5 hours, and then dried at 110 degrees Celsius for 1 hour to obtain a modified filler; wherein the weight ratio of the carbon nanotubes to the aluminum hydroxide is 1:2; the weight ratio of the modifying liquid to the mixture is 1:13.5.
[0027] Preparation Example 4 Preparation Example 4 provides a method for preparing a modified filler, comprising the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified liquid; wherein the weight ratio of the organic solvent, water and γ-aminopropyltriethoxysilane is 18:2:5; the organic solvent is ethanol; The carbon nanotubes and aluminum hydroxide are stirred and mixed evenly to obtain a mixture. Then, while stirring the mixture, the modifying liquid is slowly sprayed into the mixture. After the spraying is completed, the mixture is stirred for 0.5 hours, and then dried at 110 degrees Celsius for 1 hour to obtain a modified filler; wherein the weight ratio of the carbon nanotubes to the aluminum hydroxide is 1:2; the weight ratio of the modifying liquid to the mixture is 1:14.
[0028] Preparation Example 5 Preparation Example 5 provides a method for preparing a modified filler, comprising the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified liquid; wherein the weight ratio of the organic solvent, water and γ-aminopropyltriethoxysilane is 18:2:5; the organic solvent is ethanol; The carbon nanotubes and aluminum hydroxide are stirred and mixed evenly to obtain a mixture. Then, while stirring the mixture, the modifying liquid is slowly sprayed into the mixture. After the spraying is completed, the mixture is stirred for 0.5 hours, and then dried at 110 degrees Celsius for 1 hour to obtain a modified filler; wherein the weight ratio of the carbon nanotubes to the aluminum hydroxide is 1:2; the weight ratio of the modifying liquid to the mixture is 1:14.5. Example
[0029] Example 1 Embodiment 1 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 20 kg of silicone rubber, 5 kg of vinyl silicone oil, 5 kg of the modified filler in Preparation Example 1, 1 kg of phenolic resin, 10 kg of a cross-linking agent, 5 kg of a foaming agent, and 0.5 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0030] Example 2 Embodiment 2 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 20 kg of silicone rubber, 5 kg of vinyl silicone oil, 5 kg of the modified filler in Preparation Example 2, 1 kg of phenolic resin, 10 kg of a cross-linking agent, 5 kg of a foaming agent, and 0.5 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0031] Example 3 Embodiment 3 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 20 kg of silicone rubber, 5 kg of vinyl silicone oil, 5 kg of the modified filler in Preparation Example 3, 1 kg of phenolic resin, 10 kg of a cross-linking agent, 5 kg of a foaming agent, and 0.5 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0032] Example 4 Embodiment 4 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 20 kg of silicone rubber, 5 kg of vinyl silicone oil, 5 kg of the modified filler in Preparation Example 4, 1 kg of phenolic resin, 10 kg of a cross-linking agent, 5 kg of a foaming agent, and 0.5 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0033] Example 5 Embodiment 5 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 20 kg of silicone rubber, 5 kg of vinyl silicone oil, 5 kg of the modified filler in Preparation Example 5, 1 kg of phenolic resin, 10 kg of a cross-linking agent, 5 kg of a foaming agent, and 0.5 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0034] Example 6 Embodiment 6 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 25 kg of silicone rubber, 7.5 kg of vinyl silicone oil, 10 kg of the modified filler in Preparation Example 3, 3 kg of phenolic resin, 12.5 kg of a cross-linking agent, 7.5 kg of a foaming agent, and 0.8 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0035] Example 7 Embodiment 7 provides a method for preparing a high temperature resistant flame retardant foam, comprising the following steps: 30 kg of silicone rubber, 10 kg of vinyl silicone oil, 15 kg of the modified filler in Preparation Example 3, 5 kg of phenolic resin, 15 kg of a cross-linking agent, 10 kg of a foaming agent, and 1 kg of a catalyst were stirred and mixed to obtain a crude material; wherein the silicone rubber is α, ω-dihydroxy polysiloxane; the cross-linking agent is hydrogen-containing silicone oil; the foaming agent is a mixture of sodium ricinoleate and dimethyl silicone oil, and the weight ratio of sodium ricinoleate to dimethyl silicone oil is 1:1; the catalyst is a platinum catalyst; The coarse material is added into a silicone extruder for extrusion molding to obtain a silicone core; the molded silicone core is pulled into a dryer and dried at 50°C for 5 minutes; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam; wherein the conductive layer is a copper-plated layer.
[0036] Example 8 The difference between Example 8 and Example 6 is that the foaming agent is sodium ricinoleate; the remaining steps are consistent with Example 6.
[0037] Example 9 The difference between Example 9 and Example 6 is that 25 kg of silicone rubber, 7.5 kg of vinyl silicone oil, 10 kg of the modified filler in Preparation Example 3, 3 kg of phenolic resin, 12.5 kg of cross-linking agent, 7.5 kg of foaming agent, 0.8 kg of catalyst, and 6 kg of melamine polyphosphate are stirred and mixed uniformly to obtain a coarse material; the remaining steps are consistent with Example 6.
[0038] Example 10 The difference between Example 10 and Example 9 is that 25 kg of silicone rubber, 7.5 kg of vinyl silicone oil, 10 kg of modified filler in Preparation Example 3, 3 kg of phenolic resin, 12.5 kg of cross-linking agent, 7.5 kg of foaming agent, 0.8 kg of catalyst, 6 kg of melamine polyphosphate, 7.8 kg of wollastonite powder, and 7.5 kg of talc are stirred and mixed uniformly to obtain a coarse material; the remaining steps are consistent with Example 9.
[0039] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that 26 kg of silicone rubber, 5 kg of vinyl silicone oil, 10 kg of cross-linking agent, 5 kg of foaming agent and 0.5 kg of catalyst are stirred and mixed uniformly to obtain a crude material; the remaining steps are consistent with Example 1.
[0040] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that 25 kg of silicone rubber, 5 kg of vinyl silicone oil, 1 kg of phenolic resin, 10 kg of cross-linking agent, 5 kg of foaming agent and 0.5 kg of catalyst are stirred and mixed uniformly to obtain a crude material; the remaining steps are consistent with Example 1.
[0041] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that 20 kg of silicone rubber, 5 kg of vinyl silicone oil, 5 kg of filler, 1 kg of phenolic resin, 10 kg of cross-linking agent, 5 kg of foaming agent and 0.5 kg of catalyst are stirred and mixed uniformly to obtain a coarse material; wherein the filler is a mixture of carbon nanotubes and aluminum hydroxide, and the weight ratio of carbon nanotubes to aluminum hydroxide is 1:2; and the remaining steps are consistent with Example 1.
[0042] Performance testing (1) High temperature resistance: Using a TGA 5500 analyzer, 6 mg of the sample powder was transferred to a platinum pan and tested at a heating rate of 10°C / min under a nitrogen flow. The test temperature was increased from room temperature to 500°C, and the mass loss at 500°C was obtained. The smaller the mass loss, the better the high temperature resistance of the foam.
[0043] (2) Flame retardant properties: The high temperature resistant flame retardant foam in each embodiment was cut open, and the foam inside was tested according to "GB-T2406.2-2009 Oxygen Index Method for Determination of Combustion Behavior of Plastics" to obtain the oxygen index A. The higher the oxygen index A, the better the flame retardant property of the foam.
[0044] Table 1 Foam performance test results In combination with Example 1 and Comparative Examples 1-3, the high temperature resistance and flame retardant properties of the foam in Example 1 are the best. It can be seen that when preparing the rough material, phenolic resin and γ-aminopropyltriethoxysilane-modified filler are added to the raw material, the carbon nanotubes in the filler have good thermal conductivity, and aluminum hydroxide will decompose at high temperature to produce water, and then the phenolic resin is used to improve the high temperature resistance and flame retardant properties of the foam.
[0045] Combined with Examples 1-5, the foams in Examples 2-4 have good high temperature resistance and flame retardancy. It can be seen that when preparing the modified filler, the ratio of the modified liquid to the mixed material is preferably 1:(13-14), and the performance of the modified filler is better, thereby finally obtaining a foam with good high temperature resistance and flame retardancy.
[0046] Combining Example 3, Example 6 and Example 7, the high temperature resistance and flame retardant properties of the foam in Example 6 are the best. It can be seen that when preparing the coarse material, the amount of raw materials used is increased, and the high temperature resistance and flame retardant properties of the foam finally obtained show a trend of first increasing and then decreasing.
[0047] Combining Example 6 and Example 8, the foam in Example 6 has better high temperature resistance and flame retardant properties. It can be seen that when preparing the coarse material, the foaming agent is preferably a mixture of sodium ricinoleate and dimethyl silicone oil, and the obtained foam has better performance.
[0048] Combining Example 6 and Example 9, the flame retardant properties of the foam in Example 9 are better, which shows that when preparing the coarse material, adding melamine polyphosphate to the raw material can further improve the flame retardant properties of the final foam.
[0049] Combining Example 9 and Example 10, the high temperature resistance of the foam in Example 10 is better. It can be seen that when preparing the coarse material, wollastonite powder and talcum powder are added to the raw materials. Both wollastonite powder and talcum powder have good high temperature resistance, and talcum powder can also make the raw materials in the base layer evenly dispersed, thereby further improving the high temperature resistance of the foam.
[0050] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high temperature resistant flame retardant foam, comprising a base layer and a conductive layer, characterized in that: The raw materials of the base layer include the following components in parts by weight: 20-30 parts of silicone rubber, 5-10 parts of vinyl silicone oil, 5-15 parts of modified filler, 1-5 parts of phenolic resin, 10-15 parts of cross-linking agent, 5-10 parts of foaming agent, and 0.5-1 part of catalyst; the raw materials of the modified filler include γ-aminopropyltriethoxysilane, organic solvent, carbon nanotubes, and aluminum hydroxide.
2. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The preparation method of the modified filler comprises the following steps: Firstly add water to the organic solvent, then add γ-aminopropyltriethoxysilane, stir and mix evenly to obtain a modified solution; The carbon nanotubes and aluminum hydroxide are stirred and mixed evenly to obtain a mixture, and then the modified liquid is sprayed into the mixture while stirring the mixture. After the spraying is completed, the mixture is continuously stirred and dried to obtain a modified filler.
3. The high temperature resistant flame retardant foam according to claim 2, characterized in that: The weight ratio of the modified liquid to the mixed material is 1:(13-14).
4. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The crosslinking agent includes hydrogen-containing silicone oil.
5. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The foaming agent comprises a mixture of sodium ricinoleate and dimethyl silicone oil.
6. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The catalyst includes a platinum catalyst.
7. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The raw materials of the base layer also include 5 to 7 parts by weight of melamine polyphosphate.
8. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The raw materials of the base layer also include 5 to 10 parts by weight of wollastonite powder and 5 to 10 parts by weight of talc powder.
9. The high temperature resistant flame retardant foam according to claim 1, characterized in that: The conductive layer is a copper-plated layer and a gold-plated layer.
10. A method for preparing the high temperature resistant flame retardant foam according to claims 1-9, characterized in that: The following steps are involved: The silicone rubber, vinyl silicone oil, modified filler, phenolic resin, crosslinking agent, foaming agent, catalyst and other raw materials are stirred and mixed uniformly to obtain a coarse material; The coarse material is extruded and formed to obtain a silicone core; the formed silicone core is pulled into a dryer for drying; a conductive layer is compounded on the outer wall of the dried silicone core, and the core is cut to obtain a high temperature resistant flame retardant foam.
Citation Information
Patent Citations
Oil-resistant high-temperature-resistant seal gasket rubber for cylinders and preparation method thereof
CN104829889A
High-performance conductive rubber composite material and preparation method thereof
CN106810878A
Buffering and damping shielding foam and preparation method thereof
CN115304905A
Flame-retardant conductive foam and preparation process thereof
CN115534456A
Conductive foam and preparation method thereof
CN116278259A