Biodegradable barrier composite film doped with two-dimensional mica and preparation method thereof
By using water bath heating and ultrasonic treatment of mica powder and organic acid solution, two-dimensional mica nanosheets were prepared and blended with PBAT and corn starch, which solved the uncontrollable gas barrier properties and degradation rate of the PBAT/TPS composite film. Problem, efficient gas barrier and biodegradation control is achieved.
Patent Information
- Application Number
- CN202411011932.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing PBAT/TPS composite film has poor gas barrier properties and its degradation rate cannot be regulated, which limits its application in agricultural plastic film and food film packaging.
By performing water bath heat treatment of mica powder and organic acid solution, the two-dimensional mica nanosheets are peeled off by ultrasonic waves and melt blended with PBAT and corn starch, a biodegradable barrier doped with two-dimensional mica is prepared by hot pressing treatment. Composite film.
The gas barrier properties and mechanical properties of the composite film are improved, while the biodegradation rate can be adjusted and the degradation time is extended.
Smart Images

Figure CN118909314A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano biodegradable composite materials, and in particular relates to a biodegradable barrier composite film doped with two-dimensional mica and a preparation method thereof. Background Art
[0002] Polybutylene adipate / terephthalate (PBAT) has become one of the most popular biodegradable materials on the market due to its good impact resistance, flexibility and heat resistance. Thermoplastic starch (TPS) is a biodegradable material. It is modified from corn starch, cassava starch, sweet potato starch and other starches by plasticizers. It is widely used in packaging bags, tableware, 3D printing and other fields due to its low price, good flexibility and biodegradability. By blending and modifying PBAT and TPS, a PBAT / TPS composite material with the advantages of PBAT and TPS can be obtained. However, the gas barrier properties of PBAT and TPS are poor, and the degradation rate of PBAT / TPS composite film cannot be controlled, which is far from enough for the preparation of some agricultural mulch and gas barrier food film packaging, limiting the expansion of the application range of PBAT / TPS composite film. Therefore, it is crucial to further improve the gas barrier properties and biodegradability of PBAT / TPS composite film.
[0003] Adding two-dimensional nanomaterials to PBAT / TPS composite materials to improve their gas barrier properties is one of the commonly used methods. At present, there are literature reports that adding graphene, montmorillonite, etc. to biodegradable composite materials can improve the gas barrier properties of biodegradable composite materials and reduce the degradation rate of biodegradable composite materials. Mica is a layered silicate material whose main component is silicon dioxide (SiO2). Natural mica has a tightly stacked layered structure due to the internal van der Waals force, and it is difficult to peel off a few layers of two-dimensional mica nanosheets.
[0004] Therefore, how to simply and efficiently obtain the exfoliated two-dimensional nano-mica material and simultaneously improve the gas barrier properties, mechanical properties and regulate the biodegradation rate of the biodegradable composite film is a problem to be solved. Summary of the invention
[0005] In view of this, the present invention discloses a biodegradable barrier composite film doped with two-dimensional mica and a preparation method thereof. The biodegradable composite film prepared by the method of the present invention not only has excellent gas barrier properties and mechanical properties, but also can effectively regulate the biodegradation rate of the composite film.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The first technical purpose of the present invention is to provide a method for preparing a biodegradable barrier composite film doped with two-dimensional mica, comprising the following steps:
[0008] a. After high-temperature calcination of mica powder, the mica powder is mixed with an organic acid solution and heated in a water bath, and then subjected to ultrasonication, filtration and freeze-drying to obtain organic acid-exfoliated two-dimensional mica nanosheets;
[0009] b. melt blending the two-dimensional mica nanosheets (Mica) stripped by organic acid in step a and poly (butylene adipate / terephthalate) (PBAT), corn starch, glycerol and organic acid to obtain a two-dimensional mica biodegradable composite material (PBAT / TPS / Mica);
[0010] c. The two-dimensional mica sheet biodegradable composite material is subjected to heat pressing to obtain the two-dimensional mica-doped biodegradable barrier composite film.
[0011] It should be noted that the two-dimensional exfoliated mica nanosheets described in step a are obtained by mixing calcined heat-treated mica powder with an organic acid, heating it in a water bath to cause an esterification reaction to weaken the van der Waals force between mica layers, and then subjecting it to ultrasonic treatment.
[0012] Moreover, the organic acid used in step a not only acts as an auxiliary agent to weaken the van der Waals force between mica layers, but also acts as a coupling agent between the mica sheets and the PBAT / TPS composite material, thereby achieving efficient stripping of the two-dimensional nano-mica sheets (Mica) and simultaneous improvement of the mechanical properties and gas barrier properties of the PBAT / TPS / Mica composite film.
[0013] Optionally, in step a, the mass ratio of the mica powder to the organic acid is 1:(1-4); the mass concentration of the organic acid solution is 100 mg / mL-250 mg / mL; and the organic acid is selected from one or more combinations of lactic acid, tartaric acid, citric acid, salicylic acid, malic acid, oxalic acid, quinic acid, and ethylenediaminetetraacetic acid.
[0014] Furthermore, the temperature of the high-temperature calcination treatment of the mica powder is 600°C-900°C, and the time is 30min-120min; the temperature of the water bath heating treatment of the organic acid-exfoliated mica powder is 80°C-95°C, and the time is 60min-180min; the ultrasonic power during the ultrasonic treatment is 200-600W, and the ultrasonic time is 130min-120min.
[0015] Optionally, in step b, the mass ratio of PBAT, corn starch and glycerol is 1:1-3.5:0.25-1, the mass fraction of the organic acid-exfoliated two-dimensional mica nanosheets in the composite material is 0.5wt%-5wt% of the total mass of poly (butylene adipate / terephthalate) PBAT and corn starch; the amount of organic acid added is 0.1wt%-2wt% of the total mass of the composite material, and the organic acid in step b is the same as the organic acid in step a, and is one or more combinations of lactic acid, tartaric acid, citric acid, salicylic acid, malic acid, oxalic acid, quinic acid, and ethylenediaminetetraacetic acid. .
[0016] Furthermore, in the melt blending process, the banburying mixing parameters include: banburying temperature of 130° C.-150° C., banburying speed of 35 rpm-60 rpm, and banburying time of 7 min-15 min.
[0017] Optionally, in step c, the temperature of the hot pressing treatment is 140° C.-150° C., and the hot pressing pressure is 10 MPa-15 MPa.
[0018] It is worth noting that in the preparation method of the two-dimensional mica biodegradable composite film provided by the present invention, the van der Waals force between the mica layers is weakened by the esterification reaction of organic acid, and then a few-layer two-dimensional mica nanosheets are peeled off by ultrasonic treatment, so that the two-dimensional mica nanosheets have the characteristics of large sheet diameter; adding a few-layer two-dimensional mica nanosheets can extend the permeation path of gas through the biodegradable composite film, thereby improving the gas barrier performance of the two-dimensional mica biodegradable composite film; at the same time, the two-dimensional mica nanosheets modified by organic acid stripping have good compatibility with the PBAT / TPS composite material, thereby improving the mechanical properties of the two-dimensional mica biodegradable composite film; the two-dimensional mica nanosheets have certain antibacterial properties, and the addition of two-dimensional mica nanosheets is conducive to regulating the degradation rate of the two-dimensional mica biodegradable composite film, thereby more flexibly controlling the degradation time of the biodegradable composite film.
[0019] The second technical purpose of the present invention is to provide a biodegradable barrier composite film doped with two-dimensional mica prepared by the above method.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention heats mica powder and an organic acid solution in a water bath to obtain two-dimensional mica nanosheets by exfoliation; the two-dimensional mica nanosheets exfoliated by organic acid are melt-blended with poly(butylene adipate / terephthalate), corn starch, glycerol and an organic acid, and an esterification reaction is performed to obtain a uniformly dispersed, reinforced and toughened two-dimensional mica sheet composite material; the composite material is subjected to a hot-pressing treatment to obtain a two-dimensional mica sheet biodegradable composite film. The two-dimensional mica sheet biodegradable composite film prepared by the present invention not only has excellent mechanical properties and adjustable biodegradability, but also has high gas barrier properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0023] Figure 1 This is an atomic force microscope image of the two-dimensional mica nanosheet prepared by the present invention.
[0024] Figure 2 It is a comparison chart of water vapor transmission (WVT) of the two-dimensional mica sheet biodegradable composite film prepared by the present invention.
[0025] Figure 3 This is an optical picture of the biodegradation process of the two-dimensional mica sheet biodegradable composite film prepared by the present invention. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0028] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0029] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0030] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0031] The invention discloses a method for preparing a biodegradable barrier composite film doped with two-dimensional mica.
[0032] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0033] Example 1: Preparation of two-dimensional mica biodegradable composite film
[0034] (1) 10 g of crude mica was placed in a muffle furnace and calcined at 800° C. for 1 hour; 10 g of the calcined crude mica was mixed with 40 g of citric acid and stirred evenly, and then 250 mL of deionized water was added to make the organic acid concentration 160 mg / mL. After reflux stirring at 90° C. for 3 hours, the mixture was filtered and washed to neutrality, and then dried in an oven at 60° C. for 12 hours; 2 g of the dried mica was dispersed in 50 mL of ethanol solution, ultrasonicated at 400 W for 2 hours using an ultrasonic cell disruptor, and allowed to stand for 48 hours; the supernatant of the mica ethanol solution after standing for 48 hours was filtered using a microporous filter membrane to obtain two-dimensional mica nanosheets, and then freeze-dried in a freeze dryer for 12 hours to obtain a two-dimensional mica nanosheet sample.
[0035] (2) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60 °C for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g), two-dimensional mica nanosheets (7 g) and citric acid (1.75 g) in a high-speed mixer for multiple times, with each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set to 140 °C, the rotor speed was 40 rpm, and the mixing time was 12 min to obtain a two-dimensional mica sheet biodegradable composite material.
[0036] (3) The obtained two-dimensional mica sheet biodegradable composite material is prepared into a two-dimensional mica sheet biodegradable composite film by a flat-plate vulcanizer at 145° C. and a pressure of 10 MPa.
[0037] Example 2: Preparation of two-dimensional mica biodegradable composite film
[0038] (1) 10 g of crude mica was placed in a muffle furnace and calcined at 800° C. for 1 hour; 10 g of the calcined crude mica was mixed with 40 g of lactic acid and stirred evenly, and then 250 mL of deionized water was added to make the organic acid concentration 160 mg / mL. After reflux stirring at 90° C. for 3 hours, the mixture was filtered and washed to neutrality, and then dried in an oven at 60° C. for 12 hours; 2 g of the dried mica was dispersed in 50 mL of ethanol solution, ultrasonicated at 400 W for 2 hours using an ultrasonic cell disruptor, and allowed to stand for 48 hours; the supernatant of the mica ethanol solution after standing for 48 hours was filtered using a microporous filter membrane to obtain two-dimensional mica nanosheets, and then freeze-dried in a freeze dryer for 12 hours to obtain a two-dimensional mica nanosheet sample.
[0039] (2) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60 °C for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g), two-dimensional mica nanosheets (7 g) and lactic acid (1.75 g) in a high-speed mixer for multiple times, with each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set to 140 °C, the rotor speed was 40 rpm, and the mixing time was 12 min to obtain a two-dimensional mica sheet biodegradable composite material.
[0040] (3) The obtained two-dimensional mica sheet biodegradable composite material is prepared into a two-dimensional mica sheet biodegradable composite film by a flat-plate vulcanizer at 145° C. and a pressure of 10 MPa.
[0041] Example 3: Preparation of two-dimensional mica biodegradable composite film
[0042] (1) 10 g of crude mica was placed in a muffle furnace and calcined at 800° C. for 1 hour; 10 g of the calcined crude mica was mixed with 40 g of ethylenediaminetetraacetic acid and stirred evenly, and then 250 mL of deionized water was added to make the organic acid concentration 160 mg / mL. After reflux stirring at 90° C. for 3 hours, the mixture was filtered and washed to neutrality, and then dried in an oven at 60° C. for 12 hours; 2 g of the dried mica was dispersed in 50 mL of ethanol solution, ultrasonicated at 400 W for 2 hours using an ultrasonic cell disruptor, and allowed to stand for 48 hours; the supernatant of the mica ethanol solution after standing for 48 hours was filtered using a microporous filter membrane to obtain two-dimensional mica nanosheets, and then freeze-dried in a freeze dryer for 12 hours to obtain a two-dimensional mica nanosheet sample.
[0043] (2) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60 °C for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g), two-dimensional mica nanosheets (7 g) and ethylenediaminetetraacetic acid (1.75 g) in a high-speed mixer for multiple times, with each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set to 140 °C, the rotor speed was 40 rpm, and the mixing time was 12 min to obtain a two-dimensional mica sheet biodegradable composite material.
[0044] (3) The obtained two-dimensional mica sheet biodegradable composite material is prepared into a two-dimensional mica sheet biodegradable composite film by a flat plate vulcanizer at 145°C and a pressure of 10 MPa.
[0045] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following experimental examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.
[0046] Comparative Example 1: Preparation of biodegradable composite film without two-dimensional mica sheets
[0047] (1) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60° C. for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g) and citric acid (1.75 g) in a high-speed mixer for multiple times, each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set at 140° C., the rotor speed was 40 rpm, and the banburying time was 12 min to obtain a mica-free biodegradable composite material.
[0048] (2) The obtained mica-free biodegradable composite material is prepared into a mica-free biodegradable composite film by a flat-plate vulcanizer at 145° C. and a pressure of 10 MPa.
[0049] Comparative Example 2: Preparation of biodegradable composite film without two-dimensional mica sheets
[0050] (1) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60° C. for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g) and lactic acid (1.75 g) in a high-speed mixer for multiple times, each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set at 140° C., the rotor speed was 40 rpm, and the banburying time was 12 min to obtain a mica-free biodegradable composite material.
[0051] (2) The obtained mica-free biodegradable composite material is prepared into a mica-free biodegradable composite film by a flat-plate vulcanizer at 145° C. and a pressure of 10 MPa.
[0052] Comparative Example 3: Preparation of biodegradable composite film without two-dimensional mica sheets
[0053] (1) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60° C. for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g) and ethylenediaminetetraacetic acid (1.75 g) in a high-speed mixer for multiple times, each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set at 140° C., the rotor speed was 40 rpm, and the banburying time was 12 min to obtain a mica-free biodegradable composite material.
[0054] (3) The obtained mica-free biodegradable composite material is prepared into a mica-free biodegradable composite film by a flat-plate vulcanizer at 145° C. and a pressure of 10 MPa.
[0055] Comparative Example 4: Preparation of biodegradable mica powder composite film
[0056] (1) 147 g corn starch and 140 g PBAT were dried in a vacuum drying oven at 60° C. for 12 h, and then the dried corn starch and PBAT were mixed with glycerol (63 g), mica powder (7 g) and citric acid (1.75 g) in a high-speed mixer for multiple times, each mixing time being 30 s; the mixture was placed in a Haake torque rheometer for melt blending, the temperature was set to 140° C., the rotor speed was 40 rpm, and the banburying time was 12 min to obtain a mica powder biodegradable composite material.
[0057] (2) The obtained mica powder biodegradable composite material is prepared into a mica powder biodegradable composite film by a flat-plate vulcanizer at 145° C. and a pressure of 10 MPa.
[0058] (1) Mechanical properties of PBAT / TPS composites, mica powder biodegradable composites and two-dimensional mica sheet biodegradable composites are shown in Table 1:
[0059] Table 1
[0060] Tensile strength(MPa) Elastic modulus (MPa) Example 1 5.92±0.38 24.88±3.01 Example 2 5.61±0.42 22.31±1.05 Example 3 5.27±0.34 19.34±1.46 Comparative Example 1 3.02±0.21 19.03±2.18 Comparative Example 2 3.02±0.18 18.97±3.04 Comparative Example 3 3.28±0.26 16.28±2.03 Comparative Example 4 5.79±0.42 22.53±2.80
[0061] It can be seen from Table 1 that after adding mica powder / two-dimensional mica sheets, the tensile strength of the biodegradable composite material is improved and the elastic modulus is maintained to a certain extent. The tensile strength and elastic modulus of the biodegradable composite film with 2wt% mica powder increased by about 92% and 18%, respectively. The tensile strength and elastic modulus of the biodegradable composite film with 2wt% citric acid-exfoliated two-dimensional mica powder further increased by about 96% and 31%, respectively.
[0062] (2) The thickness and diameter of the two-dimensional mica flakes obtained by citric acid stripping in Example 1 are as follows: Figure 1 As shown. Figure 1 It can be seen that the thickness of the two-dimensional mica flakes after exfoliation is ≤6nm, and the flake diameter is 1.5-2.5μm, which indicates that the exfoliated mica is a few-layer mica flake with a large flake diameter / thickness ratio.
[0063] (3) Comparison of water vapor permeability of PBAT / TPS composites, mica powder biodegradable composites and two-dimensional mica sheet biodegradable composites, such as Figure 2 shown.
[0064] pass Figure 2 It can be seen that the addition of mica powder and mica flakes can reduce the gas barrier properties of the film, while the two-dimensional mica flakes stripped by organic acid can further optimize the gas barrier properties of the film. The water vapor permeability of the PBAT / TPS composite film is 121.5 (g / m 2 .24h), the water vapor permeability of the mica powder biodegradable composite film is 97.3 (g / m 2 .24h), the water vapor permeability of the two-dimensional mica biodegradable composite films stripped by citric acid, lactic acid and EDTA was 87.1, 86.2 and 87.3 (g / m 2 .24h). Therefore, the addition of 2wt% organic acid-exfoliated two-dimensional mica flakes significantly improved the water vapor permeability of the PBAT / TPS composite film and optimized the gas barrier properties of the film.
[0065] (4) Optical images of the biodegradation process of PBAT / TPS composites, mica powder biodegradable composites and two-dimensional mica flake biodegradable composites, such as Figure 3 shown.
[0066] pass Figure 3 It can be seen that the addition of two-dimensional mica nanosheets can regulate the degradation rate of biodegradable composites. When the PBAT / TPS composite film was degraded in the soil for one month, cracks appeared on the surface; in the second month, the cracks increased and a large number of black spots appeared on the surface; in the third month, the film became significantly thinner and began to break locally, and its surface structure gradually loosened. The organic acid-exfoliated two-dimensional mica biodegradable composite material changed slightly in the first month; spots caused by microbial erosion appeared in the second month; cracks were observed in the third month and the film color tended to yellow.
[0067] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a biodegradable barrier composite film doped with two-dimensional mica, characterized in that: The following steps are involved: a. After high-temperature calcination of mica powder, the mica powder is mixed with an organic acid solution and heated in a water bath, and then subjected to ultrasonication, filtration and freeze-drying to obtain organic acid-exfoliated two-dimensional mica nanosheets; b. melt blending the two-dimensional mica nanosheets (Mica) stripped by organic acid in step a and poly (butylene adipate / terephthalate) (PBAT), corn starch, glycerol and organic acid to obtain a two-dimensional mica biodegradable composite material (PBAT / TPS / Mica); c. The two-dimensional mica sheet biodegradable composite material is subjected to heat pressing to obtain the two-dimensional mica-doped biodegradable barrier composite film.
2. The method for preparing the biodegradable barrier composite film doped with two-dimensional mica according to claim 1, characterized in that: In step a, the mass ratio of the mica powder to the organic acid is 1:(1-4); the mass concentration of the organic acid solution is 100 mg / mL-250 mg / mL; and the organic acid is selected from one or more combinations of lactic acid, tartaric acid, citric acid, salicylic acid, malic acid, oxalic acid, quinic acid, and ethylenediaminetetraacetic acid.
3. The method for preparing the biodegradable barrier composite film doped with two-dimensional mica according to claim 1 or 2, characterized in that: The temperature of the high-temperature calcination treatment of the mica powder is 600°C-900°C, and the time is 30min-120min; the temperature of the water bath heating treatment of the organic acid-exfoliated mica powder is 80°C-95°C, and the time is 60min-180min; the ultrasonic power during the ultrasonic treatment is 200-600W, and the ultrasonic time is 30min-120min.
4. The method for preparing the biodegradable barrier composite film doped with two-dimensional mica according to claim 1, characterized in that: In step b, the mass ratio of PBAT, corn starch and glycerol is 1:1-3.5:0.25-1, and the mass fraction of the two-dimensional mica nanosheets stripped by the organic acid in the composite material is 0.5wt%-5wt% of the total mass of poly(adipate / butylene terephthalate) and corn starch; the amount of the organic acid added is 0.1wt%-2wt% of the total mass of the composite material, and the organic acid is the same as the organic acid in step a, which is one or more combinations of lactic acid, tartaric acid, citric acid, salicylic acid, malic acid, oxalic acid, quinic acid, and ethylenediaminetetraacetic acid.
5. The method for preparing the biodegradable barrier composite film doped with two-dimensional mica according to claim 1 or 4, characterized in that: The parameters of the banburying mixing in the melt blending process include: a banburying temperature of 130° C.-150° C., a banburying speed of 35 rpm-60 rpm, and a banburying time of 7 min-15 min.
6. The method for preparing the biodegradable barrier composite film doped with two-dimensional mica according to claim 1, characterized in that: In step c, the temperature of the hot pressing treatment is 140° C.-150° C., and the hot pressing pressure is 10 MPa-15 MPa.
7. A biodegradable barrier composite film doped with two-dimensional mica prepared by the method according to any one of claims 1 to 6.