Rubber tube rubber material containing liquid regenerated rubber and preparation method of rubber tube rubber material

By preparing waste rubber into liquid recycled rubber and adding it to rubber, the single problem of recycling and utilization of waste rubber rubber hose is solved, the closed-loop utilization of resources and environmentally friendly hose production is achieved, and the economic value and performance of the hose is improved.

CN118909330APending Publication Date: 2024-11-08宿迁绿金人橡塑机械有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411172540.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has a single recycling method for waste rubber hoses, low utilization rate, and lacks effective recycling methods, resulting in waste of resources and environmental pollution.

Method used

Using the preparation method of hose rubber containing liquid regenerated rubber, waste hose is used as raw material, and treated through intensive refining and twin screw extruder, high-quality liquid recycled rubber is prepared, and mixed into the rubber to form recycled rubber. pipes realize closed-loop use and resource utilization of waste hose.

Benefits of technology

It improves the economic value of waste hose, reduces the production cost of hose, enhances compatibility and dispersion with raw rubber, reduces the problem of poor tear resistance, and provides an environmentally friendly recycling method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a rubber tube rubber material containing liquid regenerated rubber and a preparation method thereof, and belongs to the field of waste rubber recycling, the rubber tube rubber material comprises the following raw materials by weight: 30-55 parts of natural rubber, 15-40 parts of styrene butadiene rubber, 20-35 parts of butadiene rubber, 25-40 parts of liquid regenerated rubber, 25-45 parts of carbon black, 2.5-5.5 parts of zinc oxide, 0.5-3 parts of stearic acid, 0.5-2 parts of a first anti-aging agent, and 2-4 parts of a second anti-aging agent, 2-6 parts of sulfur and 2-5 parts of an accelerant; the liquid regenerated rubber is firstly prepared from the waste rubber tube, and the liquid regenerated rubber is added into the rubber tube rubber material, so that the rubber tube rubber material has good compatibility and dispersity, the use amount of carbon black is reduced, the use amount of raw rubber is saved, and the rubber tube rubber material has remarkable economic and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a hose rubber compound containing liquid recycled rubber and a preparation method thereof. Background Art

[0002] Rubber can be seen everywhere in industrial production and life, and its application range is also very wide. Correspondingly, a lot of rubber waste will be generated. How to effectively utilize my country's waste rubber resources has been studied by many people in various aspects. The recycling of waste rubber is not only to protect the ecological environment and alleviate the shortage of rubber resources in my country, but also an inevitable measure to build a resource-saving and environmentally friendly society. It has far-reaching strategic significance.

[0003] In my country, the main use of rubber at present is to make tires. In 2020, the amount of waste tires generated in my country reached 370 million, about 13.5 million tons, while the total amount of other waste rubber products was only 1.5 million tons. Therefore, rubber products other than tires have not received enough attention, and the methods of recycling and reuse are relatively single.

[0004] Rubber is also widely used in hoses, such as mud-water mixture hoses in water conservancy projects, water hoses and cement slurry hoses used in construction projects, hydraulic hoses used in engineering machinery, gas hoses and oil and liquid chemical hoses used in petrochemicals, and underground and underwater rubber protective sleeves, etc. The effective recycling and reuse of these rubber hoses is also of great significance to environmental protection and alleviating the shortage of rubber resources. Summary of the invention

[0005] The present invention provides a hose rubber compound containing liquid regenerated rubber and a preparation method thereof, in an effort to solve or at least alleviate at least one of the above problems.

[0006] The present invention provides a method for preparing a hose rubber compound containing liquid regenerated rubber, the preparation method comprising:

[0007] Add natural rubber, styrene-butadiene rubber, butadiene rubber, liquid recycled rubber, stearic acid, zinc oxide, the first antioxidant, and the second antioxidant into an internal mixer, mix for 40 to 60 seconds, add carbon black when the temperature rises to 115 to 140° C., mix for another 50 to 80 seconds, and discharge to obtain a mixed rubber when the temperature rises to 150 to 170° C.;

[0008] The mixed rubber is conveyed to a twin-screw extruder via a continuous feeding device, the screw speed of the twin-screw extruder is controlled at 80-150 rpm, the temperature is controlled at 5-20° C., and the rubber is extruded when the temperature of the rubber reaches 10-35° C., and the aspect ratio of the screw of the twin-screw extruder is (40-48):1;

[0009] The obtained rubber material, sulfur and accelerator are added into an internal mixer and mixed for 50 to 80 seconds. When the temperature rises to 80 to 100° C., the material is discharged to obtain the hose rubber material.

[0010] As a preferred embodiment of the present invention, the method for preparing the liquid regenerated rubber comprises:

[0011] The waste rubber powder, softener and activator are added into an internal mixer at a weight ratio of 100:(3-8):(2-6), and then kneaded for 3-5 minutes. The waste rubber powder is then fed into a twin-screw extruder through a continuous feeding device. The temperature of different sections of the twin-screw extruder is controlled at 240°C-320°C in a closed oxygen-proof environment to react for 2-7 minutes. The waste rubber powder is then fed into a filter device with a mesh size of 80-120 to remove impurities in the rubber material. The liquid regenerated rubber is obtained after cooling, wherein the sol content is greater than 75% and the number average molecular weight Mn is 6000-18000.

[0012] As a preferred embodiment of the present invention, the waste rubber powder comprises: the recycled waste rubber tube is cleaned and crushed to obtain waste rubber powder of 20 to 60 meshes.

[0013] As a preferred embodiment of the present invention, the softener includes: any one or more combinations of environmentally friendly aromatic oil, pine tar asphalt, and tall oil asphalt, and the activator includes: any one or more combinations of aromatic disulfide and aniline sulfide regeneration activators.

[0014] As a preferred embodiment of the present invention, the first antioxidant includes antioxidant RD.

[0015] As a preferred embodiment of the present invention, the second antioxidant includes one of antioxidant AW, antioxidant 4010, and antioxidant 4010NA.

[0016] As a preferred embodiment of the present invention, the accelerator includes any one or more combinations of accelerator CZ and accelerator DZ.

[0017] As a preferred embodiment of the present invention, the proportions of each material are 30-55 parts by weight of natural rubber, 15-40 parts of styrene-butadiene rubber, 20-35 parts of butadiene rubber, 25-40 parts of liquid recycled rubber, 20-45 parts of carbon black, 2.5-5.5 parts of zinc oxide, 0.5-3 parts of stearic acid, 0.5-2 parts of the first antioxidant, 0.5-4 parts of the second antioxidant, 2-6 parts of sulfur, and 2-5 parts of accelerator, wherein the total number of parts of the natural rubber, the styrene-butadiene rubber and the butadiene rubber is 100 parts.

[0018] The invention provides a hose rubber material containing liquid regenerated rubber, and the hose rubber material is prepared by the preparation method of the hose rubber material containing liquid regenerated rubber provided by the invention.

[0019] Compared with the prior art, the present invention has at least the following beneficial effects:

[0020] In view of the problems that the current recycling methods for waste rubber hoses are relatively single and the utilization rate is low, the present invention provides a hose rubber compound containing liquid recycled rubber and a preparation method thereof. The rubber compound uses waste rubber hoses as raw materials, and is prepared into liquid recycled rubber which is mixed in the rubber compound to prepare recycled rubber hoses, thereby realizing the recycling and closed-loop use of waste rubber hoses, and greatly improving the economic value of waste rubber hoses.

[0021] At the same time, the present invention uses waste rubber hoses as the raw material for liquid recycled rubber. The prepared liquid recycled rubber can replace part of raw rubber as the raw material for preparing rubber hoses. It has better compatibility with raw rubber and better dispersibility. It not only realizes the recycling and resource utilization of waste rubber hoses, but also reduces the production cost of rubber hoses, which is more energy-saving and environmentally friendly. In the process of preparing liquid recycled rubber, a closed oxygen-proof environment is ensured to avoid the presence of oxygen, reduce the oxidation of rubber, and promote the three-dimensional network structure of most rubber hydrocarbons to break and become short-chain hydrocarbons. When used with raw rubber, it can achieve a plasticizing effect similar to that of aromatic oil. The addition of recycled rubber prepared by the traditional desulfurization process to raw rubber will cause the binding force between macromolecules to weaken, resulting in large flex cracks in the products after mixing. At the same time, due to the substantial degradation of the main chain and the cross-linking bonds, the number average molecular weight of the obtained liquid recycled rubber is between 9000 and 17000. The original additives in the waste rubber are easier to disperse when the liquid recycled rubber is used together with the raw rubber, which effectively reduces the problems such as poor tear resistance caused by uneven dispersion of the compounding agents when adding recycled rubber; providing a more environmentally friendly method to solve the problem of recycling waste rubber hoses. DETAILED DESCRIPTION

[0022] Exemplary embodiments of the present invention will be described in more detail below. Although exemplary embodiments of the present invention have been shown, it should be appreciated that the present invention can be realized in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to more thoroughly understand the present invention, and the scope of the present invention can be fully communicated to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0023] Example 1

[0024] The composition is composed of the following ingredients by weight:

[0025]

[0026]

[0027] The preparation of the liquid regenerated rubber used in this embodiment 1 comprises the following steps:

[0028] 1) The recycled waste rubber tube is cleaned and crushed to obtain 24-mesh waste rubber powder.

[0029] 2) Add the waste rubber powder, softener and activator in a weight ratio of 100:3:3, put them into the internal mixer and mix them for 3 minutes before discharging. The softener is environmentally friendly aromatic oil and the activator is B450.

[0030] 3) The rubber compound obtained by mixing is fed into a twin-screw extruder through a continuous feeding device. In a closed oxygen-proof environment, the temperature of different sections of the extruder is controlled at 240° C. to 320° C., and the rubber compound is reacted for 4 minutes under the action of heat and high shear of the screw. The rubber compound is then fed to a filter device with a mesh size of 80 to remove impurities in the rubber compound. After cooling, liquid regenerated rubber is obtained, and the sol content of the liquid regenerated rubber is 76% and the number average molecular weight is 9852.

[0031] The method for preparing the hose compound comprises the following steps:

[0032] 1) Add the above materials into an internal mixer in the order of natural rubber, styrene-butadiene rubber, butadiene rubber, liquid recycled rubber, stearic acid, zinc oxide, the first antioxidant, and the second antioxidant, mix for 45 seconds, add carbon black when the temperature rises to 115°C, mix for 60 seconds, and discharge the rubber to obtain a mixed rubber when the temperature rises to 155°C.

[0033] 2) The mixed rubber is conveyed to a twin-screw extruder via a continuous feeding device, the screw speed is controlled at 115 rpm, the temperature is at 7°C, the aspect ratio of the screw is 42:1, and when the temperature of the rubber reaches 18°C, it is extruded into sheets.

[0034] 3) Add the rubber material, sulfur and accelerator obtained in step 2) into an internal mixer and mix for 58 seconds. When the temperature reaches 77° C., discharge the material to obtain the hose rubber material. Remove the sheet from the mixer, cool and stack it.

[0035] Example 2

[0036] A hose compound containing liquid reclaimed rubber, the compound comprising the following components in parts by weight:

[0037]

[0038] The preparation of liquid recycled rubber includes the following steps:

[0039] 1) The recycled waste rubber tube is cleaned and crushed to obtain 32-mesh waste rubber powder.

[0040] 2) Add the waste rubber powder, softener and activator in a weight ratio of 100:4:3, put them into an internal mixer and mix them for 4 minutes before discharging. The softener is environmentally friendly aromatic oil and the activator is B480.

[0041] 3) The rubber compound obtained by mixing is fed into a twin-screw extruder through a continuous feeding device. In a closed oxygen-proof environment, the temperature of different sections of the extruder is controlled at 240° C. to 320° C., and the rubber compound is reacted for 5 minutes under the action of heat and high shear of the screw. The rubber compound is then fed to a filter device with a mesh number of 100 to remove impurities in the rubber compound. After cooling, liquid regenerated rubber is obtained, and the sol content of the liquid regenerated rubber is 79% and the number average molecular weight is 10166.

[0042] The preparation method of the above hose rubber material comprises the following steps:

[0043] 1) Add the above materials into the internal mixer in the order of natural rubber, styrene-butadiene rubber, butadiene rubber, liquid recycled rubber, stearic acid, zinc oxide, the first antioxidant, and the second antioxidant, mix for 48 seconds, add carbon black when the temperature reaches 119°C, mix for 63 seconds, and discharge the rubber when the temperature rises to 158°C.

[0044] 2) The mixed rubber is conveyed to a twin-screw extruder via a continuous feeding device, the screw speed is controlled at 124 rpm, the temperature is at 9°C, the aspect ratio of the screw is 44:1, and when the temperature of the rubber reaches 16°C, it is extruded into sheets.

[0045] 3) Add the rubber material, sulfur and accelerator obtained in step 2) into an internal mixer and mix for 67 seconds. When the temperature reaches 83° C., discharge the material to obtain the hose rubber material. Remove the sheet from the mixer, cool and stack it.

[0046] Example 3

[0047] A hose compound containing liquid reclaimed rubber, the compound comprising the following components in parts by weight:

[0048]

[0049] The preparation of liquid recycled rubber includes the following steps:

[0050] 1) The recovered waste rubber tubes are cleaned and crushed to obtain 30-mesh waste rubber powder.

[0051] 2) The waste rubber powder, softener and activator were added in a weight ratio of 100:5:2, and put into an internal mixer for internal mixing for 4 minutes before discharging. The softener was tall oil asphalt, and the activator was 980.

[0052] 3) The rubber compound obtained by mixing is fed into a twin-screw extruder through a continuous feeding device. In a closed oxygen-proof environment, the temperature of different sections of the extruder is controlled at 240° C. to 320° C., and the rubber compound is reacted for 6 minutes under the action of heat and high shear of the screw. The rubber compound is then fed to a filter device with a mesh size of 120 to be filtered to remove impurities in the rubber compound. After cooling, liquid regenerated rubber is obtained, and the sol content of the liquid regenerated rubber is 81% and the number average molecular weight is 11327.

[0053] The preparation method of the above hose rubber material comprises the following steps:

[0054] 1) Add the above materials into the internal mixer in the order of natural rubber, styrene-butadiene rubber, butadiene rubber, liquid recycled rubber, stearic acid, zinc oxide, antioxidant 1, and antioxidant 2, mix for 50 seconds, add carbon black when the temperature reaches 126°C, mix for 65 seconds, and discharge the rubber when the temperature rises to 163°C.

[0055] 2) The mixed rubber is conveyed to a twin-screw extruder via a continuous feeding device, the screw speed is controlled at 136 rpm, the temperature is 10°C, the aspect ratio of the screw is 44:1, and when the temperature of the rubber reaches 19°C, it is extruded into sheets.

[0056] 3) Add the rubber material, sulfur and accelerator obtained in step 2) into an internal mixer and mix for 73 seconds. When the temperature reaches 87° C., discharge the material to obtain the hose rubber material. Remove the sheet from the mixer, cool and stack it.

[0057] Comparative Example 1

[0058] A hose compound containing recycled rubber, the compound comprising the following components in parts by weight:

[0059]

[0060] The above-mentioned mixing method of the rubber material comprises the following steps:

[0061] 1) Add the above materials into the internal mixer in the order of natural rubber, styrene-butadiene rubber, butadiene rubber, recycled rubber, stearic acid, zinc oxide, the first antioxidant, and the second antioxidant, mix for 52 seconds, add carbon black when the temperature reaches 120°C, mix for 60 seconds, and discharge the rubber when the temperature rises to 153°C.

[0062] 2) The mixed rubber is conveyed to a twin-screw extruder via a continuous feeding device, the screw speed is controlled at 128 rpm, the temperature is 10°C, the aspect ratio of the screw is 44:1, and when the temperature of the rubber reaches 17°C, it is extruded into sheets.

[0063] 3) Add the rubber obtained in step 2), sulfur and accelerator into an internal mixer and mix for 68 seconds. When the temperature reaches 82° C., discharge the material, remove the sheet from the mixer, cool and stack.

[0064] The results of the above-mentioned Example 1, Example 2, Example 3 and the comparative example are shown in the following table:

[0065] Vulcanization: 140℃×20min Example 1 Example 2 Example 3 Comparative Example 1 Tensile strength / MPa 21.8 22.1 22.3 20.5 300% elongation / MPa 11.2 11.4 11.5 10.8 Elongation at break / % 527 531 536 518 Hardness / Shore A 62 62 63 60

[0066] It should be understood that in order to streamline the present invention and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, or description thereof. However, this method of invention should not be interpreted as reflecting the intention that the claimed invention requires more features than those explicitly recited in each claim. More specifically, as reflected in the claims below, inventive aspects lie in less than all of the features of a single embodiment of the preceding invention. Therefore, the claims that follow the specific embodiment are hereby expressly incorporated into the specific embodiment, with each claim itself serving as a separate embodiment of the present invention.

[0067] In addition, those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and form different embodiments. For example, in the claims, any one of the claimed embodiments may be used in any combination.

[0068] The above description is only an illustrative embodiment of the present invention and is not intended to limit the present invention in any form or substance. It should be pointed out that, for ordinary technicians in this technical field, a number of improvements and supplements made without departing from the method of the present invention should also be regarded as the protection scope of the present invention; any equivalent changes, modifications and evolutions made by technicians familiar with this profession using the technical content disclosed above without departing from the spirit and scope of the present invention are all equivalent embodiments of the present invention; at the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention still fall within the protection scope of the present invention.

Claims

1. A method for preparing a hose rubber compound containing liquid recycled rubber, characterized in that: The preparation method comprises: Add natural rubber, styrene-butadiene rubber, butadiene rubber, liquid recycled rubber, stearic acid, zinc oxide, the first antioxidant, and the second antioxidant into an internal mixer, mix for 40 to 60 seconds, add carbon black when the temperature rises to 115 to 140° C., mix for another 50 to 80 seconds, and discharge to obtain a mixed rubber when the temperature rises to 150 to 170° C.; The mixed rubber is conveyed to a twin-screw extruder via a continuous feeding device, the screw speed of the twin-screw extruder is controlled at 80-150 rpm, the temperature is controlled at 5-20° C., and the rubber is extruded when the temperature of the rubber reaches 10-35° C., and the aspect ratio of the screw of the twin-screw extruder is 40-48:1; The obtained sulfur, accelerator and the rubber material are added into an internal mixer and mixed for 50 to 80 seconds. When the temperature rises to 80 to 100° C., the material is discharged to obtain the hose rubber material.

2. The method for preparing a hose rubber compound containing liquid regenerated rubber according to claim 1, characterized in that: The preparation method of the liquid regenerated rubber comprises: The waste rubber powder, softener and activator are added into an internal mixer in a weight ratio of 100:3-8:2-6, and mixed for 3-5 minutes, and then fed into a twin-screw extruder through a continuous feeding device; the temperature of different sections of the twin-screw extruder is controlled in a closed oxygen-proof environment, and reacted at 240°C-320°C for 2-5 minutes; the waste rubber powder is fed into a filter device with a mesh number of 80-120 to filter and remove impurities in the rubber material, and the liquid regenerated rubber is obtained after cooling, wherein the sol content of the liquid regenerated rubber is greater than 75% and the number average molecular weight Mn is 6000-18000.

3. The method for preparing a hose compound containing liquid regenerated rubber according to claim 2, characterized in that: The waste rubber powder comprises the waste rubber powder of 20 to 60 meshes obtained by washing and crushing the recycled waste rubber tube.

4. The method for preparing a hose compound containing liquid regenerated rubber according to claim 2, characterized in that: The softener includes: environmentally friendly aromatic oil 、 Any one or more combinations of pine tar pitch and tall oil pitch; the activator includes: any one or more combinations of aromatic disulfide and aniline sulfide regeneration activators.

5. The method for preparing a hose compound containing liquid regenerated rubber according to claim 1, characterized in that: The first antioxidant includes antioxidant RD.

6. The method for preparing a hose compound containing liquid regenerated rubber according to claim 1, characterized in that: The second antioxidant includes one of antioxidant AW, antioxidant 4010, and antioxidant 4010NA.

7. The method for preparing a hose compound containing liquid regenerated rubber according to claim 1, characterized in that: The accelerator includes any one or more combinations of accelerator CZ and accelerator DZ.

8. The method for preparing a hose compound containing liquid regenerated rubber according to any one of claims 1 to 7, characterized in that: The proportions of each material in parts by weight are 30-55 parts of natural rubber, 15-40 parts of styrene-butadiene rubber, 20-35 parts of butadiene rubber, 25-40 parts of liquid recycled rubber, 20-45 parts of carbon black, 2.5-5.5 parts of zinc oxide, 0.5-3 parts of stearic acid, 0.5-2 parts of the first antioxidant, 2-4 parts of the second antioxidant, 2-6 parts of sulfur, and 2-5 parts of accelerator, wherein the total number of parts of the natural rubber, the styrene-butadiene rubber and the butadiene rubber is 100 parts.

9. A hose compound containing liquid recycled rubber, characterized in that: The hose rubber compound is prepared by the method for preparing a hose rubber compound containing liquid regenerated rubber according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Tire side rubber material utilizing regenerated rubber as well as blending method and application thereof

    CN101628992A

  • Liquid reclaimed rubber-containing conveyor belt cover rubber material and preparation method thereof

    CN113150413A

  • Tire tread rubber material containing liquid reclaimed rubber and preparation method thereof

    CN113278207A

  • Rubber composition for passenger car tire

    JP2002265685A

  • Natural rubber / styrene-butadiene rubber-based composition, and rubber conveyer belt using the same

    JP2004250564A