PVC (polyvinyl chloride) foamed sheet as well as preparation method and application thereof
Through the synergistic effect of the modified AC foaming agent and N-lauryl diethanolamine, the problem of high density and insufficient mechanical properties of the hard PVC foamed sheet is solved, and the preparation of PVC foamed sheet with low density and good mechanical properties is achieved. Suitable for interior decoration and furniture manufacturing.
Patent Information
- Application Number
- CN202410973431.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The hard PVC high foamed plates prepared in the prior art have problems of high density and insufficient mechanical properties, and the large addition of fillers will reduce the mechanical properties of the PVC plates.
Using modified AC foaming agent, the compatibility and decomposition temperature of AC foaming agent with PVC resin are improved by coating polymethyl methacrylate with azodiformamide and synergistically with N-lauryl diethanolamine. Consistent, form stable foam, improve foaming ratio and mechanical properties.
PVC foamed plates with low density and excellent mechanical properties were prepared, with high foaming ratio and low density, and significantly improved mechanical properties (such as average bending strength, freeze-thaw resistance, plate-side screw force, Shore hardness) were significantly improved.
Smart Images

Figure BDA0004953879520000101 
Figure BDA0004953879520000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fine chemical industry, and in particular to a PVC foaming plate and a preparation method and application thereof. Background Art
[0002] Polyvinyl chloride (PVC) resin is a polar non-crystalline polymer. Its products have good physical and chemical properties and can be widely used in industries, construction, agriculture and daily necessities. According to the amount of additives used, it is divided into soft and hard polyvinyl chloride. Soft products are soft and tough, and feel sticky; hard products have a higher hardness than low-density polyethylene, but lower than polypropylene. They are widely used in the fields of plates, pipes, soles, toys, doors and windows, wire sheaths, stationery, etc. At present, there are many varieties of modified PVC materials, which are mainly modified according to the application performance of the materials. For example, using fillers such as calcium carbonate, talcum powder and other modified PVC can reduce production costs; PVC foam materials made with foaming agents can be used as building decoration, flooring, furniture materials, etc. PVC foam board is a new type of plastic board developed in foreign countries in the 1970s. It has a series of characteristics such as waterproof, flame retardant, acid and alkali resistance, moth-proof, heat preservation, and sound insulation. It is an ideal substitute for wood, aluminum, and composite boards. It is widely used in construction, vehicle and ship manufacturing, furniture, flooring, outdoor flower box railings, fences, pavilions and other places. It is a major trend of replacing wood with plastic for environmental sustainable development and circular economy.
[0003] PVC is an amorphous white powder with a small degree of branching and a relative density of 1.35 to 1.46 g / cm 3 , the glass transition temperature is 77-90℃, and it starts to decompose at around 170℃. It has poor stability to light and heat. It will decompose to produce hydrogen chloride at above 100℃ or after long-term exposure to sunlight, and further autocatalytic decomposition will cause discoloration, and the physical and mechanical properties will also decline rapidly. In practical applications, stabilizers must be added to improve the stability to heat and light. Heat stabilizers include free basic lead salts, such as tribasic lead sulfate, dibasic lead phosphite, and dibasic lead stearate; metal soaps, such as zinc stearate, calcium stearate, lead stearate, barium stearate, and cadmium stearate; organic tin, such as di-n-octyltin dithioacetate, dimethyl dithioacetate, di-n-butyltin dilaurate, and di-n-octyltin dilaurate; composite stabilizers, such as liquid calcium zinc barium zinc stabilizer, liquid calcium zinc stabilizer, and liquid potassium zinc stabilizer.
[0004] According to the classification of the method of generating pores, there are three main foaming methods: chemical foaming, physical foaming and mechanical foaming. The chemical foaming method is to generate gas by adding a foaming agent that is easily decomposed by heat or undergoes a chemical reaction to release gas to form uniform pores to obtain a foaming material. Commonly used thermally decomposed foaming agents include azodicarbonamide (AC), AIBN, NaHCO3, etc., and the gases released include carbon dioxide, nitrogen and ammonia. AC foaming agent has the advantages of large gas emission, non-toxic and odorless decomposition products, and easy dispersion in the resin melt. It is the foaming agent with the widest application field and the largest consumption in China. For example, the Korean patent with publication number KR20120064906A discloses a PVC foamed coated yarn and a floor material containing the foamed coated yarn. The foamed coated yarn contains 100 parts of polyvinyl chloride resin, 30-80 parts of plasticizer, 1-8 parts of stabilizer, and 1-5 parts of foaming agent, wherein the foaming agent is AC foaming agent.
[0005] Commonly used stabilizers contain lead salts or zinc salts, which have an activation effect on AC foaming agents, thereby reducing the decomposition temperature of AC foaming agents from the original 195°C to 130-170°C. The foaming principle of foamed products is that the plasticization speed of the resin must match the decomposition speed of the foaming agent to achieve a high foaming rate. In order to obtain a sheet with a high foaming rate and a low specific gravity, the plasticization speed of the PVC resin must be synchronized with the decomposition of azodicarbonamide, otherwise the foaming rate and specific gravity of the product will be difficult to meet the standards. Therefore, in order to synchronize the decomposition of the activated AC foaming agent and meet the foaming rate, when the decomposition temperature of the AC foaming agent is reduced, SG8 type PVC resin powder with a lower plasticization temperature is often used as the base material. However, the SG8 type PVC resin has a low degree of polymerization, a small molecular weight, and insufficient mechanical strength, which makes the mechanical strength of the produced PVC foam board insufficient.
[0006] Most of the rigid PVC foam materials that have been industrially produced in my country are low-foaming products, generally formed by extrusion foaming, with a density of 500-1000kg / m 3. In addition, the foaming ratio of ordinary rigid PVC foam boards in China is low, and high-foaming PVC materials are mainly concentrated in soft PVC. However, low-foaming board products have high density and weight, which brings inconvenience during use and transportation. Therefore, the preparation of rigid and lightweight foamed boards has become a research hotspot. For example, the Chinese patent with publication number CN102408645A discloses a formula and a method for making a PVC foam board, which mainly improves the hardness by adding calcium carbonate and talcum powder, and uses azobisisobutyronitrile as the main foaming agent, AC and sodium bicarbonate as auxiliary foaming agents to improve the foaming ratio; the Chinese patent with publication number CN106009372A discloses a formula and a method for making a rigid PVC high-foaming board, which improves the hardness of the foamed board by adding fillers such as calcium carbonate, talcum powder, magnesium sulfate or potassium titanate. However, the large addition of fillers will reduce the mechanical properties of PVC boards.
[0007] The invention patent with the publication number CN116284977A discloses an inorganic surface-modified azodicarbonamide and its preparation method and application, wherein inorganic substances are deposited on the surface of azodicarbonamide, wherein the inner deposition layer is a silicon dioxide deposition layer or an aluminum phosphate deposition layer, and the outer deposition layer is an aluminum oxide deposition layer. The modified foaming agent can be used in rigid PVC foaming boards. The inorganic substances are used to coat azodicarbonamide, thereby blocking the contact between azodicarbonamide and the outside world, making it difficult for azodicarbonamide to decompose at high temperatures and the generated gas to escape, resulting in a decrease in the amount of gas generated, which affects the foaming effect of the PVC board.
[0008] Therefore, the rigid PVC high foamed board prepared in the prior art still has certain defects. Summary of the invention
[0009] In order to solve the above technical problems, the purpose of the present invention is to provide a PVC foamed board with low density and excellent mechanical properties, and a preparation method and application thereof; the PVC foamed board uses a modified AC foaming agent, which is prepared by coating an appropriate amount of PMMA on the AC foaming agent, thereby improving the compatibility of the AC foaming agent with the PVC resin and improving the consistency of the foam density; at the same time, PMMA can protect the AC foaming agent, ensuring that the decomposition temperature of the AC foaming agent is basically consistent with the plasticization temperature of the PVC resin, thereby facilitating the formation of stable foam; the synergistic effect of the modified AC foaming agent and N-lauryl diethanolamine makes the generated foam delicate and stable, so that the foaming ratio of the PVC board is high and the density of the prepared PVC board is low.
[0010] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0011] On one hand, the present invention provides a PVC foamed board, which comprises the following raw materials in parts by weight: 100 parts of PVC resin, 3-6 parts of foaming agent, 10-20 parts of filler, 1-3 parts of plasticizer, 6-10 parts of stabilizer, 1-3 parts of foaming regulator, and 1-3 parts of lubricant; the foaming agent is a mixture of modified AC foaming agent and N-lauryl diethanolamine in a mass ratio of (8-10):1.
[0012] The modified AC foaming agent is prepared by coating 2 to 4 parts of polymethyl methacrylate on 100 parts of azodicarbonamide. The specific preparation method is: dissolve 2 to 4 parts of polymethyl methacrylate in an organic solvent, spray the solution into 100 parts of azodicarbonamide for mixing and dispersion, remove the solvent and dry to obtain the modified AC foaming agent. The organic solvent can be one or more of benzene, toluene, ethylene dichloride, carbon tetrachloride, chloroform and acetone, preferably toluene. Polymethyl methacrylate is a polymer of methyl methacrylate with a density of 1.15 to 1.19 g / m 3 , melting point 150℃. If the amount of PMMA coating is too much, PMMA is difficult to melt quickly and cannot release the AC foaming agent; if the amount of PMMA coating is too little, it will not play a coating role. Coating an appropriate amount of PMMA on the AC foaming agent improves the compatibility of the AC foaming agent with the PVC resin, and can be stably dispersed in the PVC resin melt, avoiding the problem of inconsistent foam density in the resin caused by uneven dispersion of the foaming agent; at the same time, PMMA can protect the AC foaming agent, preventing other additives such as zinc salts in the stabilizer from lowering the decomposition temperature of the AC foaming agent, causing the AC foaming agent to decompose prematurely, resulting in inconsistency with the plasticization temperature of the PVC resin, and the foam cannot be cured and sealed in time after formation, thus affecting the foaming effect.
[0013] The PVC resin is at least one of suspension polymerization PVC resin, emulsion polymerization PVC resin, and bulk polymerization PVC resin, preferably suspension polymerization PVC resin; the suspension polymerization PVC resin models are SG1 to SG8, and from SG1 to SG8, the viscosity gradually decreases, the K value decreases, and the average degree of polymerization decreases, such as the viscosity of SG1 is 144-156 ml / g, the K value is 75-77, and the average degree of polymerization is 1536-1785, the viscosity of SG3 is 127-135 ml / g, the K value is 71-72, and the average degree of polymerization is 1251-1370, and the viscosity of SG8 is 73-86 ml / g, the K value is 55-59, and the average degree of polymerization is 650-740. The modified AC foaming agent is suitable for SG1-SG3 PVC resins, and more preferably SG3.
[0014] The filler is at least one of calcium carbonate, talcum powder, fly ash and glass beads, preferably light calcium carbonate.
[0015] The plasticizer is at least one of dioctyl phthalate, dibutyl phthalate and dioctyl terephthalate, preferably dioctyl phthalate.
[0016] The stabilizer is at least one of a calcium zinc stabilizer, a rare earth stabilizer, and an organic tin stabilizer, and is preferably a calcium zinc stabilizer.
[0017] The foaming regulator is an acrylic resin foaming regulator.
[0018] The lubricant is at least one of polyethylene wax, paraffin wax, metal soaps, and stearic acid, and is preferably a mixture of polyethylene wax and calcium stearate in a mass ratio of (1-2):1.
[0019] Another aspect of the present invention provides a method for preparing the PVC foamed plate, which is specifically:
[0020] 1) Weighing each raw material by weight, adding all the raw materials into a hot mixer and mixing for 10-15 minutes, the speed of the hot mixer is 1200-1500 rpm, and the temperature is 115-120° C.; then transferring to a cold mixer and cooling to 40-50° C. at a speed of 100-120 rpm, and discharging to obtain a mixed material;
[0021] 2) The mixed material is transferred to a twin-screw extruder, and the mixed material is plasticized into a melt after high-temperature heating and screw shearing; the melt is extruded by the twin-screw extruder and flows through a mold to form a plate embryo, and the plate embryo enters a shaping table for cooling after exiting the die to obtain a PVC foamed board; wherein the temperatures of the four heating zones of the twin-screw extruder are: zone 1 140-150°C, zone 2 150-170°C, zone 3 170-190°C, zone 4 190-200°C; the mold temperature is 195-205°C.
[0022] The PVC foamed board of the invention can be applied to interior decoration, furniture or floor manufacturing.
[0023] The beneficial effects of the present invention are:
[0024] The PVC foaming plate of the invention uses a modified AC foaming agent, which is prepared by coating 2 to 4 parts of polymethyl methacrylate (PMMA) on 100 parts of azodicarbonamide. A proper amount of PMMA is coated on the AC foaming agent, thereby improving the compatibility of the AC foaming agent with the PVC resin, enabling the AC foaming agent to be stably dispersed in the PVC resin melt, thereby avoiding the problem of inconsistent foam density in the resin caused by uneven dispersion of the foaming agent. Meanwhile, PMMA can protect the AC foaming agent, thereby avoiding the reduction of the decomposition temperature of the AC foaming agent due to other additives such as zinc salt in the stabilizer, thereby ensuring that the decomposition temperature of the AC foaming agent is substantially consistent with the plasticization temperature of the PVC resin, and the generated gas can be solidified and sealed in time to form a stable foam.
[0025] The synergistic effect of the modified AC foaming agent and N-lauryl diethanolamine produces fine and stable foam, improves the foaming ratio of the PVC sheet, and has a low density.
[0026] The PVC foam material prepared by the invention has low density and excellent mechanical properties (average bending strength, bending elastic modulus, freeze-thaw resistance, board surface screw holding force, Shore hardness, etc.). DETAILED DESCRIPTION
[0027] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The invention provides a PVC foaming plate, comprising the following raw materials in parts by weight: 100 parts of PVC resin, 3-6 parts of foaming agent, 10-20 parts of filler, 1-3 parts of plasticizer, 6-10 parts of stabilizer, 1-3 parts of foaming regulator and 1-3 parts of lubricant; the foaming agent is a mixture of modified AC foaming agent and N-lauryldiethanolamine in a mass ratio of (8-10):1; the modified AC foaming agent is prepared by coating 2-4 parts of polymethyl methacrylate on 100 parts of azodicarbonamide.
[0029] The specific preparation method of the modified AC foaming agent is as follows: dissolving 2 to 4 parts of polymethyl methacrylate in an organic solvent, spraying the solution into 100 parts of azodicarbonamide for mixing and dispersion, removing the solvent and drying to obtain the modified AC foaming agent.
[0030] Wherein, the PVC resin is a suspension polymerization method SG3 type PVC resin.
[0031] The filler is at least one of calcium carbonate, talcum powder, fly ash and glass beads, preferably light calcium carbonate.
[0032] The plasticizer is at least one of dioctyl phthalate, dibutyl phthalate and dioctyl terephthalate, preferably dioctyl phthalate.
[0033] The stabilizer is at least one of a calcium zinc stabilizer, a rare earth stabilizer, and an organic tin stabilizer, and is preferably a calcium zinc stabilizer.
[0034] The foaming regulator is an acrylic resin foaming regulator.
[0035] The lubricant is at least one of polyethylene wax, paraffin, metal soaps, and stearic acid; preferably, it is a mixture of polyethylene wax and calcium stearate in a mass ratio of (1-2):1.
[0036] The preparation method of the PVC foamed board is specifically as follows:
[0037] 1) Weighing each raw material by weight, adding all the raw materials into a hot mixer and mixing for 10-15 minutes, the speed of the hot mixer is 1200-1500 rpm, and the temperature is 115-120° C.; then transferring to a cold mixer and cooling to 40-50° C. at a speed of 100-120 rpm, and discharging to obtain a mixed material;
[0038] 2) The mixed material is transferred to a twin-screw extruder, and the mixed material is plasticized into a melt after high-temperature heating and screw shearing; the melt is extruded by the twin-screw extruder and flows through a mold to form a plate embryo, and the plate embryo enters a shaping table for cooling after exiting the die to obtain a PVC foamed board; wherein the temperatures of the four heating zones of the twin-screw extruder are: zone 1 140-150°C, zone 2 150-170°C, zone 3 170-190°C, zone 4 190-200°C; the mold temperature is 195-205°C.
[0039] The PVC foamed board of the invention can be used in interior decoration, furniture or floor manufacturing.
[0040] The present invention is further described in detail below through specific examples.
[0041] Preparation of modified AC foaming agent
[0042] Preparation Example 1
[0043] 3 parts by weight of polymethyl methacrylate was dissolved in toluene, and the solution was sprayed into 100 parts by weight of azodicarbonamide for mixing and dispersion. The toluene was removed and the mixture was dried to obtain a modified AC foaming agent A1.
[0044] Preparation Example 2
[0045] 2 parts by weight of polymethyl methacrylate was dissolved in toluene, and the solution was sprayed into 100 parts by weight of azodicarbonamide for mixing and dispersion. The toluene was removed and the mixture was dried to obtain a modified AC foaming agent A2.
[0046] Preparation Example 3
[0047] 4 parts by weight of polymethyl methacrylate was dissolved in toluene, and the solution was sprayed into 100 parts by weight of azodicarbonamide for mixing and dispersion. The toluene was removed and the mixture was dried to obtain a modified AC foaming agent A3.
[0048] Comparative Preparation Example 1
[0049] 1 part by weight of polymethyl methacrylate was dissolved in toluene, and the solution was sprayed into 100 parts by weight of azodicarbonamide for mixing and dispersion, and the toluene was removed and dried to obtain the modified AC foaming agent A4.
[0050] Comparative Preparation Example 2
[0051] 5 parts by weight of polymethyl methacrylate was dissolved in toluene, and the solution was sprayed into 100 parts by weight of azodicarbonamide for mixing and dispersion. The toluene was removed and the mixture was dried to obtain a modified AC foaming agent A5.
[0052] Preparation of PVC foam board
[0053] According to the raw material formula of the PVC foam board in Table 1, each component was weighed, and the PVC foam board was prepared according to the following method.
[0054] 1) Add all the raw materials into a hot mixer and mix for 15 minutes at a speed of 1200 rpm and a temperature of 120° C.; then transfer to a cold mixer and cool to 45° C. at a speed of 100 rpm, and discharge to obtain a mixed material;
[0055] 2) The mixed material is transferred to a twin-screw extruder, and the mixed material is plasticized into a melt after high-temperature heating and screw shearing; the melt is extruded by the twin-screw extruder and flows through a mold to form a plate embryo, and the plate embryo enters a shaping table for cooling after exiting the die to obtain a PVC foamed board; wherein the temperatures of the four heating zones of the twin-screw extruder are: zone 1 140-150°C, zone 2 150-170°C, zone 3 170-190°C, zone 4 190-200°C; the mold temperature is 195-205°C.
[0056] Table 1. Raw materials for PVC foam board
[0057]
[0058] Performance test of PVC foam board
[0059] The performance of PVC foam boards No. 1 to No. 10 was tested, and the test results are shown in Table 2.
[0060] Apparent density: Determine according to GB / T 6343-2009 “Determination of apparent density of foam plastics and rubber”.
[0061] Vicat softening temperature: Determined by method B50 in accordance with GB / T 1633-2000 “Determination of Vicat softening temperature (VST) of thermoplastics”.
[0062] Average flexural strength, flexural elastic modulus and freeze-thaw resistance: measured in accordance with the provisions of GB / T 24137-2009 "Wood Plastic Decorative Panels".
[0063] Board surface screw holding force: refer to "4.21 Determination of screw holding force" in GB / T 17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels" for measurement.
[0064] Shore hardness: It is measured in accordance with the provisions of GB / T 2411-2008 "Plastics and hard rubber - Determination of indentation hardness (Shore hardness) using a durometer".
[0065] Table 2. PVC foam board performance test results
[0066]
[0067] As shown in Table 2, the density of PVC foam sheets with serial numbers 1 to 4 is relatively low, less than 100 kg / m 3 ; The density of PVC foam sheets with serial numbers 5 to 10 is relatively high, greater than 300kg / m 3 .
[0068] No. 5 is an AC foaming agent coated with a small amount of PMMA (1%). The coating amount is too small and has no protective effect. The AC foaming agent decomposes prematurely to generate gas. The gas is not sealed in the PVC in time, and the gas escapes, resulting in poor foaming effect of the PVC; No. 6 is an AC foaming agent coated with an excessive amount of PMMA (5%). The coating amount is too large, and PMMA melts slowly, delaying the foaming of the AC foaming agent. Plasticization and molding are performed before a large amount of gas is generated in time; No. 7 is an AC foaming agent not coated with PMMA. Due to the influence of zinc salt, the AC foaming agent decomposes prematurely to generate gas. The gas is not sealed in the PVC in time, and the gas escapes, resulting in poor foaming effect of the PVC.
[0069] No. 8 uses a small amount of N-lauryl diethanolamine, and No. 9 uses an excessive amount of N-lauryl diethanolamine. The proportion of N-lauryl diethanolamine is not within the scope of the present invention, and the synergistic effect of the two foaming agents cannot be achieved, and the foaming effect is poor; No. 10 uses alkyl glycoside as a composite foaming agent, and the foaming effect is poor; This shows that the modified AC foaming agent of the present invention has a synergistic effect with N-lauryl diethanolamine, and the foaming effect is good.
[0070] From the PVC foam sheets No. 1, 5, 6, and 7, it can be seen that the mechanical properties (average bending strength, bending elastic modulus, freeze-thaw resistance, board surface screw holding force, and Shore hardness) of the PVC foam sheets are basically the same as those of No. 1 and No. 6, which are better than No. 5, and the performance of No. 7 is poor. This is because the different PMMA coating amounts affect the compatibility of the AC foaming agent and the PVC resin, thereby affecting the mechanical properties of the PVC foam sheet. No. 5 uses a small amount of PMMA coating, and No. 7 does not use PMMA coating, which makes the compatibility of the AC foaming agent and the PVC resin poor, resulting in poor mechanical properties of the PVC foam sheet.
[0071] In summary, the PVC foamed board prepared by the present invention has the characteristics of light weight and good mechanical properties.
[0072] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0073] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A PVC foam sheet, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of PVC resin, 3-6 parts of foaming agent, 10-20 parts of filler, 1-3 parts of plasticizer, 6-10 parts of stabilizer, 1-3 parts of foaming regulator and 1-3 parts of lubricant; the foaming agent is a mixture of modified AC foaming agent and N-lauryl diethanolamine in a mass ratio of (8-10):1; the modified AC foaming agent is prepared by coating 2-4 parts of polymethyl methacrylate on 100 parts of azodicarbonamide.
2. The PVC foamed sheet according to claim 1, It is characterized in that The specific preparation method of the modified AC foaming agent is: dissolving 2 to 4 parts of polymethyl methacrylate in an organic solvent, spraying the solution into 100 parts of azodicarbonamide for mixing and dispersion, removing the solvent and drying to obtain the modified AC foaming agent.
3. The PVC foamed sheet according to claim 1, It is characterized in that The PVC resin is a suspension polymerization SG3 type PVC resin.
4. The PVC foamed sheet according to claim 1, It is characterized in that The filler is at least one of calcium carbonate, talcum powder, fly ash and glass beads; the plasticizer is at least one of dioctyl phthalate, dibutyl phthalate and dioctyl terephthalate; the stabilizer is at least one of calcium zinc stabilizer, rare earth stabilizer and organic tin stabilizer; and the foaming regulator is an acrylic resin foaming regulator.
5. The PVC foamed sheet according to claim 1, It is characterized in that The lubricant is at least one of polyethylene wax, paraffin wax, metal soaps and stearic acid.
6. The PVC foamed sheet according to claim 5, It is characterized in that The lubricant is a mixture of polyethylene wax and calcium stearate in a mass ratio of (1-2):
1.
7. A method for preparing the PVC foamed board according to any one of claims 1 to 6, It is characterized in that The steps include: 1) Weigh each raw material by weight, add all the raw materials into a hot mixer and mix for 10-15 minutes; then transfer to a cold mixer and cool to 40-50° C. at a speed of 100-120 rpm, and discharge to obtain a mixed material; 2) The mixed material is transferred to a twin-screw extruder, and the mixed material is plasticized into a melt after high-temperature heating and screw shearing; the melt is extruded through the twin-screw extruder and flows through a mold to form a plate embryo, and the plate embryo enters a shaping table after exiting the die and is cooled to obtain a PVC foamed board.
8. The method for preparing the PVC foamed board according to claim 7, It is characterized in that The speed of the hot mixer in step 1) is 1200-1500 rpm, and the temperature is 115-120°C.
9. The method for preparing the PVC foamed board according to claim 7, It is characterized in that The temperatures of the zones of the twin-screw extruder in step 2) are: 140-150°C for zone 1, 150-170°C for zone 2, 170-190°C for zone 3, and 190-200°C for zone 4; the mold temperature is 195-205°C.
10. An application of the PVC foamed board according to any one of claims 1 to 6, It is characterized in that The PVC foamed board is used in interior decoration, furniture or floor manufacturing.