Moisturizing type ultra-light clay toy containing vitamin E and preparation method of moisturizing type ultra-light clay toy
By using polycaprolactone-based microcapsule foaming agent in ultralight clay toys, the potential problems of borax and preservatives for children's health are solved, and the toy's extension performance is improved and antibacterial properties ensure the safety and functionality of children's toys.
Patent Information
- Application Number
- CN202411062194.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The crosslinking agents and preservatives used in existing ultra-light clay toys have health risks, especially borax is harmful to children's health, and has poor prolongation performance, which can easily lead to skin irritation and breakage.
Use 6-caprolactone and high-temperature foaming agent to prepare polycaprolactone-based microcapsule foaming agent, and wrap it with vitamin E, combined with basic binder, carboxylic acid-based crosslinking filler and natural essential oil antibacterial agent, through The coordinated combination of metal coordination crosslinking and natural essential oils form a moisturizing ultra-light clay toy.
It has achieved moisturizing and hydrating effects on the skin, improved the ductility and antibacterial properties of the toys, avoided the use of toxic substances, and ensured the safety and functionality of children's toys.
Smart Images

Figure CN118909375A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of children's clay toys, and particularly relates to a moisturizing ultra-light clay toy containing vitamin E and a preparation method thereof. Background Art
[0002] Clay toys are toys made of plastic materials and are often used for children's creative and handcraft activities. Clay toys mainly include the following types: (1) Traditional clay: including plasticine (soft and reusable) and pottery (natural clay); (2) Air-dried clay: dries naturally in the air without heating or baking; (3) Homemade clay: made from simple materials such as flour, salt and water; (4) Super light clay: mainly made by mixing base material, foaming filler, plasticizer, colorant and preservative, and then extruding and shaping.
[0003] China is the world's largest toy exporter and producer, with an annual toy industry valued at 100 billion yuan. Approximately 70% of global toys are produced in China, and domestic toy consumption is also increasing. In recent years, alongside common clay toys like playdough, ultra-light clay, and space sand, a variety of "internet-famous" toys have emerged, becoming extremely popular among children. These include brightly colored "crystal clay," bubble glue, "slime," and, more recently, "fake water." These products are affordable, come in a wide variety, and enjoy significant sales both online and offline. These toys, considered handmade art and DIY, are increasingly popular with parents and children both domestically and internationally due to their potential for creative expression and strong parent-child interaction. In recent years, reports of child injuries caused by clay toys due to quality issues or improper use have become commonplace. Clay toys with shapes like "crystal clay," which frequently appear in internet-famous toys, have become particularly prevalent.
[0004] Crosslinkers used in ultralight clay toys primarily increase the stickiness between the various raw materials, allowing children to freely stick them together during play, making it easy to create various shapes. Currently, the most commonly used crosslinker is borax, which is widely used due to its low price, but it also poses serious health risks. The EU REACH regulation lists boron as a candidate for substances of very high concern (SVHC), known to have toxic effects on human reproduction, development, and the endocrine system. Boron in toys primarily comes from borax. Borax reacts with stomach acid to form boric acid, which then forms complexes with carbohydrates and proteins in the body. Excessive borax ingestion over a short period of time can cause symptoms such as nausea, vomiting, depression, convulsions, skin flushing, and circulatory failure, posing significant health risks. Overdose over a long period of time can cause cumulative multi-organ toxicity, including damage to the liver, kidneys, brain, and lungs. The toxic dose of borax for adults is 1g to 3g, the lethal dose for adults is 15g to 20g, and the lethal dose for children is 5g. According to preliminary research, boron is one of the items that poses a significant safety risk. Currently, relevant toy standards in Europe and the United States have included borax in their restricted list and set limits. In recent years, there have been numerous toy recalls due to excessive boron levels. Animal studies have shown that boron has some teratogenic potential, but there have been no reports of carcinogenicity or mutagenicity. Preservatives used in ultra-light clay, such as formaldehyde, phenol, and nitrosamines, are intended to delay microbial growth or chemical spoilage, thereby extending its shelf life. However, many preservatives are allergenic, and excessive use can easily cause skin allergies, dermatitis, and other injuries in young children.
[0005] Children with poor self-control may chew, lick, or engage in prolonged skin contact with squishy toys during play. Ultra-light clay toys are also highly sticky and can cling to children's hands and clothing. If these toys come into contact with food, the mouth, nose, or skin without washing hands after play, they can pose a potential hazard. To address the health risks of crosslinkers and preservatives, existing technologies have improved their composition.
[0006] Patent CN118063912A discloses an ultra-light clay and a preparation method thereof. The invention comprises mixing, stirring and kneading water, polyvinyl alcohol rubber powder, a preservative (isothiazolinone), CMC, a foaming agent (microsphere foaming agent), vaseline, polyvinyl chloride paste resin, polyether silicone oil, boric acid, silica, sorbitol, glycerin, latex powder, sodium polyacrylate, sodium tripolyphosphate, zinc stearate, calcium carbonate, polyethylene wax and plant color paste to obtain the ultra-light clay.
[0007] Patent CN105419192A discloses a non-toxic elastic plasticine and a preparation method thereof. The invention mixes polyvinyl alcohol, 2-methyl-4-isothiazoline-3-one (preservative), eucommia fruit, anatase titanium dioxide, guar gum, hollow microspheres, natural antibacterial substances, moisturizers, pigments and deionized water to form plasticine.
[0008] Patent CN105385172A discloses a method for preparing modified glutinous rice-based ultra-light clay. The invention uses glutinous rice residue as raw material, saccharifies and enzymatically hydrolyzes the glutinous rice residue, and then mixes and ferments it with neutral protease to produce a neutral protease hydrolysate. After decolorization, the glutinous rice protein powder is spray-dried to obtain glutinous rice protein powder, which replaces the microsphere foaming powder used in the preparation of traditional ultra-light clay. The modified glutinous rice-based ultra-light clay is then mixed with various auxiliary materials to obtain a modified glutinous rice-based ultra-light clay. The ultra-light clay is not only safe and harmless, but also will not adhere to the skin, nails, or hair during use and is easy to clean. In addition, the use of glutinous rice residue as raw material realizes waste utilization and is more economical and practical.
[0009] Patent CN112159574A discloses a titanate chelate, an environmentally friendly boron-free polymer polyvinyl alcohol-based ultra-light clay, and a preparation method thereof. The invention mixes and stirs water, polyvinyl alcohol, a titanate chelate, a pigment, a microsphere foaming agent, a lubricant, a humectant, a water-retaining agent, a surfactant, and an aqueous dispersant to obtain an environmentally friendly boron-free polymer polyvinyl alcohol-based ultra-light clay. A titanate chelate is used as a cross-linking agent to cross-link with the hydroxyl groups in the polyvinyl alcohol, causing the colloid to become larger and agglomerate, thereby improving tensile properties. The invention does not contain toxic materials such as boron.
[0010] Although the above invention avoids the use of formaldehyde preservatives and borax, isothiazolinone preservatives are highly irritating to the skin, and microsphere and microbead foaming agents have poor ductility and cannot significantly deform when subjected to stress, and are therefore easily broken or shattered.
[0011] Therefore, an ultra-light clay that is less irritating to the skin and has the function of moisturizing the skin is designed and prepared, and the ultra-light clay has good ductility, which is of great significance to improving the safety and functionality of children's toys. Summary of the Invention
[0012] In response to the shortcomings of the prior art, the present invention uses 6-caprolactone as a monomer and mixes it with a high-temperature foaming agent to prepare an oil phase. The oil phase and aqueous phase are then mixed and emulsified to produce a polycaprolactone-based microcapsule foaming agent. Vitamin E is then mixed and emulsified with the polycaprolactone-based microcapsule foaming agent to form a vitamin E-encapsulated foaming agent. The vitamin E-encapsulated foaming agent, a base adhesive, a carboxylic acid-based cross-linking filler, and a natural essential oil antibacterial agent are mixed and extruded to produce a moisturizing ultra-light clay toy. Specifically, the technical solution of the present invention includes the following:
[0013] A moisturizing ultra-light clay toy containing vitamin E, comprising the following raw materials in parts by weight:
[0014] 4-7 parts by weight of a vitamin E-encapsulated foaming agent, 25-40 parts by weight of a basic adhesive, 8-13 parts by weight of a carboxylic acid-based cross-linking filler, 0.1-1 parts by weight of anhydrous copper chloride and 5-8 parts by weight of a natural essential oil antibacterial agent.
[0015] Furthermore, the preparation method of the vitamin E-encapsulated foaming agent comprises the following steps:
[0016] S1. Preparation of oil phase: 6-caprolactone, an organic metal catalyst, a high-temperature foaming agent, toluene, and a lipophilic emulsifier are mixed, stirred, and dispersed in a mass ratio of 1:0.02-0.05:1:2-3:0.1-0.2, and then stored at 0°C to 5°C to obtain the oil phase;
[0017] S2 aqueous phase preparation: deionized water and glycerol are mixed and stirred in a mass ratio of 1:0.2-0.3 and stored at 0°C-5°C to obtain the aqueous phase;
[0018] Preparation of S3 polycaprolactone-based microcapsule foaming agent: the aqueous phase and the oil phase are mixed in a mass ratio of 1:2-3, and then dispersed at a speed of 400-500 r / min for 5-7 min, and then dispersed at a speed of 1000-1500 r / min for 15-20 min to obtain a dispersion liquid, and the dispersion liquid is heated to 150-180° C. at a heating rate of 10° C. / min under nitrogen protection, and reacted for 6-10 h to obtain the polycaprolactone-based microcapsule foaming agent;
[0019] S4 Preparation of vitamin E-encapsulated foaming agent: The polycaprolactone-based microcapsule foaming agent and vitamin E are mixed in a mass ratio of 1:3 to 5 and heated to 55°C to 60°C until completely melted, and then mixed and stirred at 1000 / min to 1500r / min for 15min to 20min in the molten state to obtain the vitamin E-encapsulated foaming agent.
[0020] Furthermore, the organic metal catalyst includes stannous 2-ethylhexanoate or aluminum sec-butoxide. The organic metal catalyst forms an active chain end with glycerol through metal ions, and the active chain end reacts with 6-caprolactone, thereby activating 6-caprolactone to form a five-membered ring transition state, making it easy to open the ring, and the opened monomers undergo condensation polymerization to form polycaprolactone with good biocompatibility.
[0021] Furthermore, the high-temperature foaming agent includes azodicarbonamide or N,N'-dinitrosopentamethylenetetramine. If a low-temperature foaming agent is used, it may decompose prematurely during the polymerization process to form polycaprolactone and lose its foaming activity.
[0022] Furthermore, the lipophilic emulsifier includes Span-60, Span-80, cetyl polyethylene glycol, polyglyceryl-3-diisostearate or polyglyceryl-6 polyricinoleate.
[0023] Furthermore, the base adhesive includes polyvinyl alcohol.
[0024] Furthermore, the carboxylic acid-based cross-linked filler includes alginic acid or carboxymethyl cellulose, and the carboxylic acid-based cross-linked filler combines the foaming agent wrapped with polyvinyl alcohol and vitamin E through the metal coordination effect of copper ions in copper chloride.
[0025] Furthermore, the natural essential oil antibacterial agent includes clove oil, rosemary oil or thyme oil, and the natural essential oil antibacterial agent needs to have high temperature resistance, otherwise the temperature of the subsequent mixing and extrusion process will cause the natural essential oil antibacterial agent to be inactivated, thereby losing its antibacterial and antiseptic effects.
[0026] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, the method comprising the following steps:
[0027] 4 to 7 parts by weight of a foaming agent wrapped in vitamin E, 25 to 40 parts by weight of a basic adhesive, 8 to 13 parts by weight of a carboxylic acid-based cross-linking filler, 0.1 to 1 part by weight of anhydrous copper chloride and 5 to 8 parts by weight of a natural essential oil antibacterial agent are mixed and extruded to obtain the moisturizing ultra-light clay toy.
[0028] Furthermore, the mixing extrusion conditions include a mixing temperature of 70° C. to 80° C. and a mixing time of 2 h to 3 h.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The present invention uses 6-caprolactone as a monomer and mixes it with a high-temperature foaming agent to form an oil phase. The oil phase is then mixed with an aqueous phase for dispersion and emulsification, followed by suspension polymerization to form a polycaprolactone-based microcapsule foaming agent with a cross-linked structure, which is then mixed with vitamin E. On the one hand, with the help of the moisturizing effect of vitamin E, the prepared ultra-light clay toy has a moisturizing effect on human skin. On the other hand, the foaming agent wrapped in vitamin E forms a metal coordination cross-linking through the copper ions in copper chloride as a cross-linking structure with the carboxylic acid-based cross-linking filler through the lone electron pair effect of oxygen on vitamin E. The synergistic cooperation of the polycaprolactone group of the cross-linked structure and the metal coordination cross-linking not only improves the ductility of the ultra-light clay toy after the foaming agent is foamed, but also the coordination effect of the copper ions and the carboxylic acid-based cross-linking filler and the synergistic cooperation of the natural essential oil antibacterial agent further improves the antibacterial property of the ultra-light clay toy.
[0031] (2) In the present invention, the aqueous phase is compounded with deionized water and glycerol. Glycerol not only helps to stabilize the mixing of the oil phase and the aqueous phase, but also serves as an organic metal catalyst to catalyze the polymerization of caprolactone to form an initiator for polycaprolactone, without the need to add additional alcohol initiators.
[0032] (3) The polycaprolactone synthesized in the present invention is used as a skeleton-wrapped foaming agent and has good biocompatibility, and the carboxylic acid-based cross-linking agent also has good biocompatibility, avoiding the toxic cross-linking agent borax used in ultra-light clay, and is environmentally friendly and safe.
[0033] (4) It can be seen from the test results and microstructure diagrams of Examples 1 to 5 that the moisturizing ultra-light clay toys prepared by the present invention are relatively full of water molecules, the product has strong ductility, no damage, and good plasticity and mildew resistance.
[0034] (5) The test results and microstructures of Comparative Examples 1 and 2 show that the use of anhydrous copper chloride or carboxylic acid-based cross-linked fillers alone may result in low compressive strength, unsatisfactory plasticity and cracking properties, poor ductility, low water molecule content, and poor antibacterial properties due to the low cross-linking density of vitamin E.
[0035] (6) It can be seen from the test results and microstructure diagram of Comparative Example 3 that without adding natural essential oil antibacterial agent, the water molecules are well maintained, but a small amount of mildew still occurs, and the antibacterial performance is poor.
[0036] (7) It can be seen from the test results and microstructure diagram of Example 4 that although the water molecules are well maintained, the removal of glycerol may lead to a decrease in the catalytic polymerization effect of the organic metal catalyst, poor cross-linking density, low compressive strength, unsatisfactory plasticity and cracking properties, and poor ductility.
[0037] (8) It can be seen from the test results and microstructure diagram of Example 5 that the direct use of high-temperature foaming agent does not form an effective cross-linking system. Whether it is compressive strength, plasticity, cracking resistance and water molecule content, or antibacterial performance, the present invention shows the worst effect.
[0038] (9) It can be seen from the test results and microstructure diagram of Example 6 that although the low-temperature foaming agent also has a foaming function, due to the high temperature during the polymerization process to form polycaprolactone, it may cause premature thermal decomposition, resulting in the loss of part of the low-temperature foaming agent, resulting in a poor final foaming effect. Although the water molecule content is good, the compressive strength and plasticity are poor, and there is some cracking and poor ductility. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1This is a microstructure diagram of Example 1 of the present invention;
[0040] Figure 2 This is a microstructure diagram of Example 2 of the present invention;
[0041] Figure 3 This is a microstructure diagram of Example 3 of the present invention;
[0042] Figure 4 This is a microstructure diagram of Example 4 of the present invention;
[0043] Figure 5 This is a microstructure diagram of Example 5 of the present invention;
[0044] Figure 6 This is a microstructure diagram of Comparative Example 1 of the present invention;
[0045] Figure 7 This is a microstructure diagram of Comparative Example 2 of the present invention;
[0046] Figure 8 This is a microstructure diagram of Comparative Example 3 of the present invention;
[0047] Figure 9 This is a microstructure diagram of Comparative Example 4 of the present invention;
[0048] Figure 10 This is a microstructure diagram of Comparative Example 5 of the present invention;
[0049] Figure 11 This is a microstructure diagram of Comparative Example 6 of the present invention. DETAILED DESCRIPTION
[0050] The following will clearly and completely describe the technical solutions of the present invention through the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making any creative efforts shall fall within the scope of protection of the present invention.
[0051] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.
[0052] Preparation Example 1:
[0053] The preparation method of the foaming agent wrapped with vitamin E specifically includes the following steps:
[0054] S1 oil phase preparation:
[0055] Weigh 200 g of 6-caprolactone, 4 g of stannous 2-ethylhexanoate, 200 g of azodicarbonamide, 400 g of toluene and 20 g of Span-60, mix them in a flask, stir and disperse them evenly, and then place them in an ice-water bath to control the temperature at 5°C to obtain an oil phase.
[0056] Preparation of S2 aqueous phase:
[0057] Weigh 200 g of deionized water and 400 g of glycerol, mix them in a beaker, stir them evenly, and then place them in an ice water bath to control the temperature at 5° C. to obtain an aqueous phase.
[0058] Preparation of S3 polycaprolactone-based microcapsule foaming agent:
[0059] Take 412g of S2 aqueous phase and slowly add it dropwise to the flask containing the oil phase in 824g of S1. The dropping time is controlled to 40s. After the addition is completed, turn on the speed of 400r / min for mixing and preliminary dispersion for 5min, and then adjust the speed to 1000r / min for further dispersion for 15min to obtain a dispersion. Place the flask in a water bath and introduce nitrogen to exhaust the air. Then set the heating rate of the water bath to 10℃ / min, heat to 150℃ at a speed of 200 / rmin, and then time the reaction for 6h. After the reaction is completed, naturally cool to room temperature, then filter to obtain a precipitate, and place the precipitate in a vacuum drying oven at 60℃ and dry it for 12h to obtain a polycaprolactone-based microcapsule foaming agent.
[0060] Preparation of S4 Vitamin E-encapsulated foaming agent:
[0061] Weigh 500 g of S3 polycaprolactone-based microcapsule foaming agent and 1500 g of vitamin E and mix them together. Then heat them to 55° C. until they are completely melted. Then, stir them at a speed of 1000 r / min for 15 minutes to obtain a vitamin E-encapsulated foaming agent.
[0062] Preparation Example 2:
[0063] The preparation method of the foaming agent wrapped with vitamin E specifically includes the following steps:
[0064] S1 oil phase preparation:
[0065] Weigh 200 g of 6-caprolactone, 6 g of stannous 2-ethylhexanoate, 200 g of azodicarbonamide, 450 g of toluene and 25 g of Span-80, mix them in a flask, stir and disperse them evenly, and then place them in an ice-water bath to control the temperature at 5°C to obtain an oil phase.
[0066] Preparation of S2 aqueous phase:
[0067] Weigh 200 g of deionized water and 450 g of glycerol, mix them in a beaker, stir them evenly, and then place them in an ice water bath to control the temperature at 5° C. to obtain an aqueous phase.
[0068] Preparation of S3 polycaprolactone-based microcapsule foaming agent:
[0069] Take 440.5g of S2 aqueous phase and slowly add it dropwise to the flask containing the oil phase in 881g of S1. The dropping time is controlled to 50s. After the addition is completed, turn on the speed of 400r / min for mixing and preliminary dispersion for 5min, and then adjust the speed to 1200r / min for further dispersion for 15min to obtain a dispersion. Place the flask in a water bath and introduce nitrogen to exhaust the air. Then set the heating rate of the water bath to 10℃ / min, heat to 160℃ at a speed of 200 / rmin, and then time the reaction for 7h. After the reaction is completed, naturally cool to room temperature, then filter to obtain a precipitate, and place the precipitate in a vacuum drying oven at 60℃ and dry it for 12h to obtain a polycaprolactone-based microcapsule foaming agent.
[0070] Preparation of S4 Vitamin E-encapsulated foaming agent:
[0071] Weigh 500 g of S3 polycaprolactone-based microcapsule foaming agent and 1500 g of vitamin E, mix them together, then heat to 55° C. until completely melted, turn on the speed of 1200 r / min and stir for 15 minutes to obtain the vitamin E-encapsulated foaming agent.
[0072] Preparation Example 3:
[0073] The preparation method of the foaming agent wrapped with vitamin E specifically includes the following steps:
[0074] S1 oil phase preparation:
[0075] Weigh 200 g of 6-caprolactone, 8 g of stannous 2-ethylhexanoate, 200 g of azodicarbonamide, 500 g of toluene and 30 g of cetyl polyethylene glycol, mix them in a flask, stir and disperse them evenly, and then place them in an ice-water bath to control the temperature at 2° C. to obtain an oil phase.
[0076] Preparation of S2 aqueous phase:
[0077] Weigh 200 g of deionized water and 500 g of glycerol, mix them in a beaker, stir them evenly, and then place them in an ice water bath to control the temperature at 2° C. to obtain an aqueous phase.
[0078] Preparation of S3 polycaprolactone-based microcapsule foaming agent:
[0079] Take 375.2g of S2 aqueous phase and slowly add it dropwise to the flask containing the oil phase in 938g of S1. The dropping time is controlled to 60s. After the addition is completed, turn on the speed of 450r / min for mixing and preliminary dispersion for 6min, and then adjust the speed to 1400r / min for further dispersion for 17min to obtain a dispersion. Place the flask in a water bath and introduce nitrogen to exhaust the air. Then set the heating rate of the water bath to 10℃ / min, heat to 170℃ at a speed of 200 / rmin, and then time the reaction for 8h. After the reaction is completed, naturally cool to room temperature, then filter to obtain a precipitate, and place the precipitate in a vacuum drying oven at 60℃ and dry it for 12h to obtain a polycaprolactone-based microcapsule foaming agent.
[0080] Preparation of S4 Vitamin E-encapsulated foaming agent:
[0081] 500 g of S3 polycaprolactone-based microcapsule foaming agent and 2000 g of vitamin E were weighed and mixed together, and then heated to 57° C. until completely melted, and then stirred at a speed of 1400 r / min for 17 minutes to obtain a vitamin E-encapsulated foaming agent.
[0082] Preparation Example 4:
[0083] The preparation method of the foaming agent wrapped with vitamin E specifically includes the following steps:
[0084] S1 oil phase preparation:
[0085] Weigh 200 g of 6-caprolactone, 10 g of aluminum sec-butoxide, 200 g of N,N'-dinitrosopentamethylenetetramine, 550 g of toluene and 35 g of polyglycerol-3-diisostearate, mix them in a flask, stir and disperse them evenly, and then place them in an ice-water bath to control the temperature at 0°C to obtain an oil phase.
[0086] Preparation of S2 aqueous phase:
[0087] Weigh 200 g of deionized water and 550 g of glycerol, mix them in a beaker, stir them evenly, and then place them in an ice water bath to control the temperature at 0° C. to obtain an aqueous phase.
[0088] Preparation of S3 polycaprolactone-based microcapsule foaming agent:
[0089] Take 398g of S2 aqueous phase and slowly add it dropwise to the flask containing the oil phase in 995g of S1. The dropping time is controlled to 70s. After the dropping is completed, turn on the speed of 500r / min for mixing and preliminary dispersion for 7min, and then adjust the speed to 1500r / min for further dispersion for 20min to obtain a dispersion. Place the flask in a water bath and introduce nitrogen to exhaust the air. Then set the heating rate of the water bath to 10℃ / min, heat to 180℃ at a speed of 200 / rmin, and then time the reaction for 9h. After the reaction is completed, naturally cool to room temperature, then filter to obtain a precipitate, and place the precipitate in a vacuum drying oven at 60℃ and dry it for 12h to obtain a polycaprolactone-based microcapsule foaming agent.
[0090] Preparation of S4 Vitamin E-encapsulated foaming agent:
[0091] Weigh 500 g of S3 polycaprolactone-based microcapsule foaming agent and 2500 g of vitamin E, mix them together, then heat to 60° C. until completely melted, turn on the speed of 1500 r / min and stir for 20 minutes to obtain the vitamin E-encapsulated foaming agent.
[0092] Preparation Example 5:
[0093] The preparation method of the foaming agent wrapped with vitamin E specifically includes the following steps:
[0094] S1 oil phase preparation:
[0095] Weigh 200 g of 6-caprolactone, 10 g of aluminum sec-butoxide, 200 g of N,N'-dinitrosopentamethylenetetramine, 600 g of toluene and 40 g of polyglycerol-6 polyricinoleate, mix them in a flask, stir and disperse them evenly, and then place them in an ice water bath to control the temperature at 0°C to obtain an oil phase.
[0096] Preparation of S2 aqueous phase:
[0097] Weigh 200 g of deionized water and 600 g of glycerol, mix them in a beaker, stir them evenly, and then place them in an ice water bath to control the temperature at 0° C. to obtain an aqueous phase.
[0098] Preparation of S3 polycaprolactone-based microcapsule foaming agent:
[0099] Take 350g of S2 aqueous phase and slowly add it dropwise to the flask containing the oil phase in 1050g of S1. The dropping time is controlled to 80s. After the addition is completed, turn on the speed of 500r / min for mixing and preliminary dispersion for 7min, and then adjust the speed to 1500r / min for further dispersion for 20min to obtain a dispersion. Place the flask in a water bath and introduce nitrogen to exhaust the air. Then set the heating rate of the water bath to 10℃ / min, heat it to 180℃ at a speed of 200 / rmin, and then time the reaction for 10h. After the reaction is completed, naturally cool it to room temperature, then filter to obtain a precipitate, and place the precipitate in a vacuum drying oven at 60℃ and dry it for 12h to obtain a polycaprolactone-based microcapsule foaming agent.
[0100] Preparation of S4 Vitamin E-encapsulated foaming agent:
[0101] Weigh 500 g of S3 polycaprolactone-based microcapsule foaming agent and 2500 g of vitamin E, mix them together, then heat to 60° C. until completely melted, turn on the speed of 1500 r / min and stir for 20 minutes to obtain the vitamin E-encapsulated foaming agent.
[0102] Example 1:
[0103] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0104] 4 parts by weight of the foaming agent coated with vitamin E of Preparation Example 1, 25 parts by weight of polyvinyl alcohol, 8 parts by weight of alginic acid, 0.1 parts by weight of anhydrous copper chloride and 5 parts by weight of clove oil were mixed, heated to 70° C. and mixed and kneaded for 2 hours, and then extruded through a mold to obtain a moisturizing ultra-light clay toy.
[0105] Example 2:
[0106] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0107] 5 parts by weight of the foaming agent coated with vitamin E of Preparation Example 2, 30 parts by weight of polyvinyl alcohol, 9 parts by weight of alginic acid, 0.2 parts by weight of anhydrous copper chloride and 6 parts by weight of clove oil were mixed, heated to 72° C., mixed and kneaded for 2 hours, and then extruded through a mold to obtain a moisturizing ultra-light clay toy.
[0108] Example 3:
[0109] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0110] 6 parts by weight of the foaming agent coated with vitamin E of Preparation Example 3, 35 parts by weight of polyvinyl alcohol, 10 parts by weight of alginic acid, 0.6 parts by weight of anhydrous copper chloride and 7 parts by weight of rosemary oil were mixed, heated to 76° C., mixed and kneaded for 2.5 hours, and then extruded through a mold to obtain a moisturizing ultra-light clay toy.
[0111] Example 4:
[0112] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0113] 7 parts by weight of the foaming agent coated with vitamin E of Preparation Example 4, 40 parts by weight of polyvinyl alcohol, 12 parts by weight of carboxymethyl cellulose, 0.8 parts by weight of anhydrous copper chloride and 8 parts by weight of rosemary oil were mixed, heated to 78° C., mixed and kneaded for 3 hours, and then extruded through a mold to obtain a moisturizing ultra-light clay toy.
[0114] Example 5:
[0115] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0116] 7 parts by weight of the foaming agent coated with vitamin E of Preparation Example 5, 40 parts by weight of polyvinyl alcohol, 13 parts by weight of carboxymethyl cellulose, 1 part by weight of anhydrous copper chloride and 8 parts by weight of thyme oil were mixed, heated to 80° C. and mixed and kneaded for 3 hours, and then extruded through a mold to obtain a moisturizing ultra-light clay toy.
[0117] Comparative Example 1:
[0118] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0119] The anhydrous cupric chloride in Example 5 was removed and the other conditions remained the same as in Example 5.
[0120] Comparative Example 2:
[0121] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0122] The carboxymethyl cellulose in Example 5 was removed and the other conditions remained the same as in Example 5.
[0123] Comparative Example 3:
[0124] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0125] The thyme oil in Example 5 was removed and the other conditions remained the same as in Example 5.
[0126] Comparative Example 4:
[0127] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0128] The glycerin in Preparation Example 5 was removed and not added, and the other conditions were kept consistent with those in Preparation Example 5. The vitamin E-encapsulated foaming agent prepared in this way replaced the vitamin E-encapsulated foaming agent in Example 5, and the other conditions were kept consistent with those in Example 5.
[0129] Comparative Example 5:
[0130] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0131] The foaming agent wrapped in vitamin E in Example 5 was replaced with N,N'-dinitrosopentamethylenetetramine, and the other conditions remained the same as in Example 5.
[0132] Comparative Example 6:
[0133] A method for preparing a moisturizing ultra-light clay toy containing vitamin E, specifically comprising the following steps:
[0134] The N,N'-dinitrosopentamethylenetetramine in Preparation Example 5 was replaced with urea, and the other conditions were consistent with those in Preparation Example 5. The vitamin E-encapsulated foaming agent prepared in this way replaced the vitamin E-encapsulated foaming agent in Example 5, and the other conditions were consistent with those in Example 5.
[0135] The moisturizing ultra-light clay toys prepared in Examples 1 to 5 and Comparative Examples 1 to 6 were respectively fixed on a mechanical properties tester. The test probe was compressed downward at a speed of 3 mm / min to 50% of the diameter of the moisturizing ultra-light clay toy to test its compressive strength (KPa). Then, the cracking, plasticity, and mildew resistance of the toys were tested in accordance with QB / T 2960-2008 Colored Clay. The results are shown in the following table:
[0136]
[0137]
[0138] The embodiments described above provide a detailed description of the technical solutions and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention, and such changes and modifications fall within the scope of the present invention as claimed.
Claims
1. A moisturizing ultra-light clay toy containing vitamin E, characterized in that: The moisturizing ultra-light clay toy comprises the following raw materials in parts by weight: 4-7 parts by weight of a foaming agent wrapped in vitamin E, 25-40 parts by weight of a basic adhesive, 8-13 parts by weight of a carboxylic acid-based cross-linking filler, 0.1-1 parts by weight of anhydrous cupric chloride and 5-8 parts by weight of a natural essential oil antibacterial agent.
2. A moisturizing ultra-light clay toy containing vitamin E according to claim 1, characterized in that: The preparation method of the vitamin E-encapsulated foaming agent comprises the following steps: S1. Preparation of oil phase: 6-caprolactone, an organic metal catalyst, a high temperature foaming agent, toluene and a lipophilic emulsifier are mixed, stirred and dispersed in a mass ratio of 1:0.02-0.05:1:2-3:0.1-0.2, and then stored in an environment of 0°C to 5°C to obtain the oil phase; S2 water phase preparation: deionized water and glycerol are mixed and stirred in a mass ratio of 1:0.2-0.3 and stored in an environment of 0°C-5°C to obtain the water phase; S3 Preparation of polycaprolactone-based microcapsule foaming agent: the water phase and the oil phase are mixed in a mass ratio of 1:2-3, and then mixed and dispersed at a speed of 400r / min-500r / min for 5min-7min, and then mixed and dispersed at a speed of 1000r / min-1500r / min for 15min-20min to obtain a dispersion liquid, and the dispersion liquid is heated to 150°C-180°C at a heating rate of 10°C / min under nitrogen protection, and reacted for 6h-10h to obtain the polycaprolactone-based microcapsule foaming agent; S4 Preparation of vitamin E-encapsulated foaming agent: The polycaprolactone-based microcapsule foaming agent and vitamin E are mixed in a mass ratio of 1:3-5 and heated to 55°C-60°C until completely melted, and then mixed and stirred at 1000 / min-1500r / min for 15min-20min in the molten state to obtain the vitamin E-encapsulated foaming agent.
3. A moisturizing ultra-light clay toy containing vitamin E according to claim 2, characterized in that: The organic metal catalyst includes stannous 2-ethylhexanoate or aluminum sec-butoxide.
4. A moisturizing ultra-light clay toy containing vitamin E according to claim 2, characterized in that: The high temperature foaming agent includes azodicarbonamide or N,N'-dinitrosopentamethylenetetramine.
5. A moisturizing ultra-light clay toy containing vitamin E according to claim 2, characterized in that: The lipophilic emulsifier includes Span-60, Span-80, cetyl polyethylene glycol, polyglyceryl-3-diisostearate or polyglyceryl-6 polyricinoleate.
6. A moisturizing ultra-light clay toy containing vitamin E according to claim 1, characterized in that: The base binder includes polyvinyl alcohol.
7. A moisturizing ultra-light clay toy containing vitamin E according to claim 1, characterized in that: The carboxylic acid-based cross-linked filler includes alginic acid or carboxymethyl cellulose.
8. A moisturizing ultra-light clay toy containing vitamin E according to claim 1, characterized in that: The natural essential oil antibacterial agent includes clove oil, rosemary oil or thyme oil.
9. A method for preparing a moisturizing ultra-light clay toy containing vitamin E as claimed in any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: 4-7 parts by weight of a foaming agent wrapped in vitamin E, 25-40 parts by weight of a basic adhesive, 8-13 parts by weight of a carboxylic acid-based cross-linking filler, 0.1-1 parts by weight of anhydrous cupric chloride and 5-8 parts by weight of a natural essential oil antibacterial agent are mixed and extruded to obtain the moisturizing ultra-light clay toy.
10. The method for preparing a moisturizing ultra-light clay toy containing vitamin E according to claim 9, characterized in that: The mixing extrusion conditions include a mixing temperature of 70° C. to 80° C. and a mixing time of 2 h to 3 h.