Carbon fiber prepreg, preparation method thereof and application of carbon fiber prepreg in fin structural member
By loading titanium dioxide on carbon nanotubes and combining with epoxy resin, the problems of uneven dispersion and insufficient binding force in composite materials are solved, and the mechanical properties and durability of carbon fiber prepregs are significantly improved. Application in complex environments.
Patent Information
- Application Number
- CN202411084892.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-08
AI Technical Summary
Carbon nanotubes are prone to agglomeration in the resin matrix and are not dispersed uniformly enough, which affects the enhancement performance of the composite material. Moreover, unmodified carbon nanotubes lack binding force in the composite material, making it difficult to use in complex environments for a long time.
Using titanium dioxide/carbon nanotube composite material, the dispersion and binding force of nanotitanium dioxide are loaded on the surface of carbon nanotubes through hydrothermal reaction of tetrabutyl titanate, multi-wall carbon nanotubes and ethanol and nitrogen atmosphere calcination technology. And the binding force with the epoxy resin is used to prepare a carbon fiber prepreg with excellent modification.
It significantly improves the dispersion and binding force of carbon nanotubes in carbon fiber prepregs, enhances the mechanical properties of composite materials, and is suitable for long-term use in complex environments, extends service life and reduces repair and replacement costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of prepregs, and in particular relates to a carbon fiber prepreg and a preparation method thereof and application thereof in a wing structure. Background Art
[0002] Carbon fiber prepreg is a strong and rigid resin-based fiber-reinforced composite material formed by bonding carbon fiber and resin together through modern technology, also known as carbon fiber prepreg. Carbon fiber prepreg combines the high strength and high modulus of carbon fiber with the good adhesion and processability of the resin matrix, making the composite material as a whole have extremely high strength and stiffness. And because of the low density of carbon fiber, the composite material made of carbon fiber prepreg has the characteristics of light weight while maintaining extremely high strength.
[0003] In the aerospace field, reducing the weight of the fuselage and wings has always been the key to improving fuel efficiency and operational benefits. Carbon fiber prepreg, with its high strength and low density, has become an ideal material for reducing the weight of wings. And the wings made of carbon fiber prepreg are not only light in weight, but also have excellent mechanical properties and fatigue resistance, which can improve the overall performance of the aircraft.
[0004] To further improve the performance of wing structures, carbon fiber prepregs can also be modified in combination with other functionalized particles to improve their overall performance. For example, carbon nanotubes have extremely high strength and stiffness. Adding them to prepregs can significantly improve the overall strength and stiffness of the composite material, which is especially important for wing parts that need to withstand large aerodynamic loads and mechanical stresses. In addition, carbon nanotubes have excellent corrosion resistance and wear resistance, which can make winglets more suitable for long-term use in complex environments and reduce the cost of repair and replacement due to corrosion and wear.
[0005] The addition of carbon nanotubes can significantly improve the tensile strength, modulus, impact resistance and other mechanical properties of prepregs and their composites, but unmodified carbon nanotubes tend to agglomerate in the resin matrix and are not evenly dispersed, which can seriously affect their reinforcing properties for composites. Therefore, in the process of preparing carbon fiber prepregs, appropriate measures need to be taken to ensure uniform dispersion and good bonding of carbon nanotubes in the matrix material. Summary of the invention
[0006] The present invention provides a carbon fiber prepreg and a preparation method thereof and application in a wing structure. The titanium dioxide / carbon nanotube composite material in the carbon fiber prepreg of the present invention has good dispersibility, strong bonding with epoxy resin, and high stability. The wing structure is prepared by using the carbon fiber prepreg of the present invention, so that the wing structure has excellent mechanical properties and is suitable for long-term use in complex environments.
[0007] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0008] A carbon fiber prepreg comprises the following raw materials in weight percentage: 55-65% carbon fiber cloth and 35-45% epoxy resin mixture;
[0009] The epoxy resin mixture comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 2.8-4.2 parts of titanium dioxide / carbon nanotube composite material, 0.01-0.05 parts of silane coupling agent, 30-35 parts of curing agent, and 0.5-1.5 parts of curing accelerator.
[0010] Preferably, the preparation method of the titanium dioxide / carbon nanotube composite material comprises the following steps:
[0011] S1: adding tetrabutyl titanate to the anhydrous ethanol while stirring the anhydrous ethanol to prepare a tetrabutyl titanate ethanol solution;
[0012] S2: uniformly mixing the oxidized carbon nanotubes with anhydrous ethanol, deionized water and glacial acetic acid to obtain a mixed liquid; then dropping a tetrabutyl titanate ethanol solution into the mixed liquid while stirring the mixed liquid, and after the dropping is completed, continuing ultrasonic treatment to obtain a treated liquid;
[0013] S3: The treated liquid is transferred to a reactor for hydrothermal reaction. After the hydrothermal reaction is completed, centrifugation, water washing, alcohol washing, and drying are performed in sequence, and then calcination is performed under a nitrogen atmosphere to obtain a titanium dioxide / carbon nanotube composite material.
[0014] Preferably, in step S1, the volume ratio of anhydrous ethanol to tetrabutyl titanate is 1-1.5:15-20; in step S2, the mass volume ratio of the oxidized carbon nanotubes to anhydrous ethanol, deionized water, and glacial acetic acid is 2.5-5 g:60-80 ml:4.5-7 ml:12-15 ml;
[0015] The volume ratio of the tetrabutyl titanate ethanol solution in step S1 to the mixed liquid in step S2 is 1:3.5-5.
[0016] Preferably, in step S2, the method for preparing oxidized carbon nanotubes comprises the following steps: placing multi-walled carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, wherein the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution is 2-3:1; then performing ultrasonic treatment for 3-8 hours while stirring, and the power of the ultrasonic treatment is 200-300W; and then centrifuging, washing with water, and drying to obtain oxidized carbon nanotubes.
[0017] Preferably, the multi-walled carbon nanotubes have an inner diameter of 5-10 nm, an outer diameter of 10-30 nm, and a length of 10-30 um.
[0018] Preferably, in step S2, the dripping time is 30-40 min; the ultrasonic treatment time is 20-30 min, and the ultrasonic treatment power is 500-1000W.
[0019] Preferably, in step S3, the temperature of the hydrothermal reaction is 150-180° C. and the time is 12-24 h;
[0020] The calcining in a nitrogen atmosphere comprises: firstly heating to 200-260° C., keeping the temperature for 0.5-1 hour, then heating to 400-430° C., keeping the temperature for 1.5-2.5 hours.
[0021] Preferably, the bisphenol A type epoxy resin is one or more of epoxy resin E-44 and E-51; the silane coupling agent is 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane or 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane;
[0022] The curing agent is one or more of D230 and D400, and the curing accelerator is DMP-30;
[0023] The carbon fiber cloth is a unidirectional carbon fiber cloth.
[0024] As a general inventive concept, the present invention provides a method for preparing the above-mentioned carbon fiber prepreg, comprising the following steps:
[0025] S1: uniformly mixing the titanium dioxide / carbon nanotube composite material and the silane coupling agent, then adding them to the epoxy resin, heating to 65-70° C. and stirring and mixing, then adding the curing agent and the curing accelerator and stirring and mixing to obtain an epoxy resin mixture;
[0026] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 65-70°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the carbon fiber cloth, and the composite is hot-pressed by a roller at a composite temperature of 70-75°C, and then cooled to prepare a carbon fiber prepreg.
[0027] As a general inventive concept, the present invention also provides an application of the above-mentioned carbon fiber prepreg or the carbon fiber prepreg prepared by the above-mentioned preparation method in a wing structure, the wing structure includes an aluminum alloy frame and a composite material skin, the cavity between the aluminum alloy frame and the composite material skin is filled with foam; the composite material skin is prepared from the carbon fiber prepreg.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The carbon fiber prepreg of the present invention is modified by a titanium dioxide / carbon nanotube composite material, which includes carbon nanotubes and nano titanium dioxide loaded on the surface of the carbon nanotubes. The nano titanium dioxide significantly enhances the roughness of the carbon nanotubes, significantly enhances the dispersion performance of the carbon nanotubes, and can be firmly embedded in the epoxy resin, which has an excellent modification effect on the fiber-reinforced resin material prepared by the prepreg. Titanium dioxide is loaded on the surface of the carbon nanotubes, and the two have a strong bonding force. Even if the prepared fiber-reinforced resin material is used for a long time or subjected to a large external force impact, the carbon nanotubes and the epoxy resin still maintain a strong bonding force, and the excellent reinforcement performance of the carbon nanotubes is maintained.
[0030] In addition, loading titanium dioxide on carbon nanotubes also achieves high dispersion of titanium dioxide in the composite material. Titanium dioxide can resist the erosion of composite materials by harsh environmental factors such as ultraviolet rays, high temperature, and humidity, and can improve the aging resistance of the composite material, thereby increasing the service life of the blade in the natural environment.
[0031] 2. When preparing the titanium dioxide / carbon nanotube composite material, the raw material used in the present invention is oxidized carbon nanotubes obtained by acid oxidation of carbon nanotubes, and the surface of the carbon nanotubes has a variety of oxygen-containing groups, so that in the subsequent preparation process, the binding force between the carbon nanotubes and the titanium dioxide can be made stronger, and the present invention can make the titanium dioxide more stably compounded with the carbon nanotubes by combining the hydrothermal reaction and the nitrogen atmosphere roasting process, and the two are not easy to separate. In addition, in the process of preparing the titanium dioxide / carbon nanotube composite material, the present invention can make the multi-walled carbon nanotubes load an appropriate amount of nano titanium dioxide by reasonably configuring the addition amount of tetrabutyl titanate, multi-walled carbon nanotubes, ethanol, etc., so that the roughness of the surface of the oxidized carbon nanotubes can be improved, and too much nano titanium dioxide can be avoided. If too much titanium dioxide is loaded, it may affect the reinforcement advantage involved in the structure of the carbon nanotube itself.
[0032] 3. The titanium dioxide / carbon nanotube composite material in the carbon fiber prepreg of the present invention has good dispersibility, strong bonding with the epoxy resin, and high stability. The carbon fiber prepreg of the present invention is used to prepare wing structural parts, which can make the wing structural parts have excellent mechanical properties and are suitable for long-term use in complex environments. DETAILED DESCRIPTION
[0033] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0034] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0035] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0036] Preparation Example 1: Preparation of Titanium Dioxide / Carbon Nanotube Composite Materials
[0037] A method for preparing a titanium dioxide / carbon nanotube composite material comprises the following steps:
[0038] S1: Preparation of oxidized carbon nanotubes: placing multi-walled carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, wherein the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution is 3:1; then performing ultrasonic treatment for 8 hours while stirring, the power of the ultrasonic treatment is 200W; then centrifuging, washing with water, and drying to obtain oxidized carbon nanotubes.
[0039] The inner diameter of the multi-walled carbon nanotube is 5-10 nm, the outer diameter is 10-30 nm, and the length is 10-30 um.
[0040] S2: adding tetrabutyl titanate to the anhydrous ethanol while stirring the anhydrous ethanol to prepare a tetrabutyl titanate ethanol solution; the volume ratio of the anhydrous ethanol to the tetrabutyl titanate is 1.5:18.
[0041] S3: Evenly mix the oxidized carbon nanotubes with anhydrous ethanol, deionized water and glacial acetic acid in a mass volume ratio of 4g:80ml:6ml:15ml to obtain a mixed liquid; then drip tetrabutyl titanate ethanol solution into the mixed liquid while stirring the mixed liquid, the dripping time is 40min, and the volume ratio of tetrabutyl titanate ethanol solution to the mixed liquid is 1:5; after the dripping is completed, continue ultrasonic treatment, the ultrasonic treatment time is 20min, the power is 1000W, and a treated liquid is obtained.
[0042] S4: The treated liquid is transferred to a reactor for hydrothermal reaction at a temperature of 170°C for 18 hours. After the hydrothermal reaction is completed, centrifugation, water washing, alcohol washing and drying are carried out in sequence. The dried material is then heated to 260°C in a nitrogen atmosphere for 0.5 hours, and then heated to 420°C for 1.5 hours to obtain a titanium dioxide / carbon nanotube composite material.
[0043] Preparation Example 2: Preparation of Titanium Dioxide / Carbon Nanotube Composite Materials
[0044] A method for preparing a titanium dioxide / carbon nanotube composite material comprises the following steps:
[0045] S1: Preparation of oxidized carbon nanotubes: placing multi-walled carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, wherein the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution is 3:1; then performing ultrasonic treatment for 3 hours while stirring, the power of the ultrasonic treatment is 300W; then centrifuging, washing with water, and drying to obtain oxidized carbon nanotubes.
[0046] The inner diameter of the multi-walled carbon nanotube is 5-10 nm, the outer diameter is 10-30 nm, and the length is 10-30 um.
[0047] S2: adding tetrabutyl titanate to the anhydrous ethanol while stirring the anhydrous ethanol to prepare a tetrabutyl titanate ethanol solution; the volume ratio of the anhydrous ethanol to the tetrabutyl titanate is 1:15.
[0048] S3: Evenly mix the oxidized carbon nanotubes with anhydrous ethanol, deionized water and glacial acetic acid in a mass volume ratio of 5g:80ml:7ml:15ml to obtain a mixed liquid; then drip tetrabutyl titanate ethanol solution into the mixed liquid while stirring the mixed liquid, the dripping time is 30min, and the volume ratio of tetrabutyl titanate ethanol solution to the mixed liquid is 1:4; after the dripping is completed, continue ultrasonic treatment, the ultrasonic treatment time is 25min, the power is 800W, and a treated liquid is obtained.
[0049] S4: The treated liquid is transferred to a reactor for hydrothermal reaction at a temperature of 180°C for 12 hours. After the hydrothermal reaction, centrifugation, water washing, alcohol washing and drying are performed in sequence. The dried material is then heated to 200°C in a nitrogen atmosphere for 1 hour, and then heated to 400°C for 2 hours to obtain a titanium dioxide / carbon nanotube composite material.
[0050] Preparation Example 3: Preparation of Titanium Dioxide / Carbon Nanotube Composite Materials
[0051] A method for preparing a titanium dioxide / carbon nanotube composite material comprises the following steps:
[0052] S1: Preparation of oxidized carbon nanotubes: placing multi-walled carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, wherein the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution is 2:1; then performing ultrasonic treatment for 6 hours while stirring, the power of the ultrasonic treatment is 300W; then centrifuging, washing with water, and drying to obtain oxidized carbon nanotubes.
[0053] The inner diameter of the multi-walled carbon nanotube is 5-10 nm, the outer diameter is 10-30 nm, and the length is 10-30 um.
[0054] S2: adding tetrabutyl titanate to the anhydrous ethanol while stirring the anhydrous ethanol to prepare a tetrabutyl titanate ethanol solution; the volume ratio of the anhydrous ethanol to the tetrabutyl titanate is 1.2:20.
[0055] S3: Evenly mix the oxidized carbon nanotubes with anhydrous ethanol, deionized water and glacial acetic acid in a mass volume ratio of 2.5g:60ml:4.5ml:12ml to obtain a mixed liquid; then drip tetrabutyl titanate ethanol solution into the mixed liquid while stirring the mixed liquid, the dripping time is 35min, and the volume ratio of tetrabutyl titanate ethanol solution to the mixed liquid is 1:3.5; after the dripping is completed, continue ultrasonic treatment, the ultrasonic treatment time is 30min, the power is 500W, and a treated liquid is obtained.
[0056] S4: The treated liquid was transferred to a reactor for hydrothermal reaction at a temperature of 150°C for 24 hours. After the hydrothermal reaction, centrifugation, water washing, alcohol washing and drying were carried out in sequence. The dried material was heated to 230°C in a nitrogen atmosphere for 1 hour, and then heated to 430°C for 2.5 hours to obtain a titanium dioxide / carbon nanotube composite material.
[0057] Embodiment 1:
[0058] A carbon fiber prepreg comprises the following raw materials in weight percentage: 60% carbon fiber cloth and 40% epoxy resin mixture;
[0059] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin E-44, 3.5 parts of titanium dioxide / carbon nanotube composite material, 0.02 parts of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 30 parts of curing agent D230, and 1 part of curing accelerator DMP-30.
[0060] The above-mentioned carbon fiber cloth is a carbon fiber unidirectional cloth, and the density of the carbon fiber unidirectional cloth is 150±1g / m 2 The titanium dioxide / carbon nanotube composite material was prepared by the method in Preparation Example 2.
[0061] The method for preparing the carbon fiber prepreg in this embodiment comprises the following steps:
[0062] S1: The titanium dioxide / carbon nanotube composite material and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane are mixed evenly, and then added to the epoxy resin E-44, heated to 70° C. and stirred and mixed, and then the curing agent D230 and the curing accelerator DMP-30 are added and stirred and mixed to obtain an epoxy resin mixture;
[0063] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 70°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the carbon fiber cloth, and the composite is hot-pressed by a roller at a composite temperature of 75°C, and then cooled to prepare a carbon fiber prepreg.
[0064] Embodiment 2:
[0065] A carbon fiber prepreg comprises the following raw materials in weight percentage: 55% carbon fiber cloth and 45% epoxy resin mixture;
[0066] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin E-44, 3.5 parts of titanium dioxide / carbon nanotube composite material, 0.03 parts of 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 32 parts of curing agent D400, and 0.8 parts of curing accelerator DMP-30.
[0067] The above-mentioned carbon fiber cloth is a carbon fiber unidirectional cloth, and the density of the carbon fiber unidirectional cloth is 150±1g / m 2 The titanium dioxide / carbon nanotube composite material was prepared by the method in Preparation Example 1.
[0068] The method for preparing the carbon fiber prepreg in this embodiment comprises the following steps:
[0069] S1: The titanium dioxide / carbon nanotube composite material and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane are mixed evenly, and then added to the epoxy resin E-44, heated to 65° C. and stirred and mixed, and then the curing agent D400 and the curing accelerator DMP-30 are added and stirred and mixed to obtain an epoxy resin mixture;
[0070] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 65°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the carbon fiber cloth, and the composite is hot-pressed by a roller at a composite temperature of 73°C, and then cooled to prepare a carbon fiber prepreg.
[0071] Embodiment 3:
[0072] A carbon fiber prepreg comprises the following raw materials in weight percentage: 65% carbon fiber cloth and 35% epoxy resin mixture;
[0073] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin E-44, 3 parts of titanium dioxide / carbon nanotube composite material, 0.03 parts of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 30 parts of curing agent D400, and 0.5 parts of curing accelerator DMP-30.
[0074] The above-mentioned carbon fiber cloth is a carbon fiber unidirectional cloth, and the density of the carbon fiber unidirectional cloth is 150±1g / m 2 The titanium dioxide / carbon nanotube composite material was prepared by the method in Preparation Example 3.
[0075] The method for preparing the carbon fiber prepreg in this embodiment comprises the following steps:
[0076] S1: The titanium dioxide / carbon nanotube composite material and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane are mixed evenly, and then added to the epoxy resin E-44, heated to 68° C. and stirred and mixed, and then the curing agent D400 and the curing accelerator DMP-30 are added and stirred and mixed to obtain an epoxy resin mixture;
[0077] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 68°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the carbon fiber cloth, and the composite is hot-pressed by a roller at a composite temperature of 70°C, and then cooled to prepare a carbon fiber prepreg.
[0078] Embodiment 4:
[0079] A carbon fiber prepreg comprises the following raw materials in weight percentage: 58% carbon fiber cloth and 42% epoxy resin mixture;
[0080] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin E-44, 4.2 parts of titanium dioxide / carbon nanotube composite material, 0.05 parts of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 30 parts of curing agent D230, and 1 part of curing accelerator DMP-30.
[0081] The above-mentioned carbon fiber cloth is a carbon fiber unidirectional cloth, and the density of the carbon fiber unidirectional cloth is 150±1g / m 2 The titanium dioxide / carbon nanotube composite material was prepared by the method in Preparation Example 3.
[0082] The preparation method of the carbon fiber prepreg in this embodiment is the same as that in Example 1.
[0083] Embodiment 5:
[0084] A carbon fiber prepreg comprises the following raw materials in weight percentage: 64% carbon fiber cloth and 36% epoxy resin mixture;
[0085] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin E-44, 3.6 parts of titanium dioxide / carbon nanotube composite material, 0.03 parts of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 32 parts of curing agent D230, and 1.2 parts of curing accelerator DMP-30.
[0086] The above-mentioned carbon fiber cloth is a carbon fiber unidirectional cloth, and the density of the carbon fiber unidirectional cloth is 150±1g / m 2 The titanium dioxide / carbon nanotube composite material was prepared by the method in Preparation Example 1.
[0087] The preparation method of the carbon fiber prepreg in this embodiment is the same as that in Example 1.
[0088] Embodiment 6:
[0089] A carbon fiber prepreg comprises the following raw materials in weight percentage: 62% carbon fiber cloth and 38% epoxy resin mixture;
[0090] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin E-44, 2.8 parts of titanium dioxide / carbon nanotube composite material, 0.01 parts of 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 35 parts of curing agent D400, and 1.5 parts of curing accelerator DMP-30.
[0091] The above-mentioned carbon fiber cloth is a carbon fiber unidirectional cloth, and the density of the carbon fiber unidirectional cloth is 150±1g / m 2 The titanium dioxide / carbon nanotube composite material was prepared by the method in Preparation Example 2.
[0092] The preparation method of the carbon fiber prepreg in this embodiment is the same as that in Example 2.
[0093] Embodiment 7:
[0094] A wing structure comprises an aluminum alloy frame and a composite material skin, wherein a cavity between the aluminum alloy frame and the composite material skin is filled with foam; the foam is polymethacrylimide foam, the aluminum alloy frame can be specifically 2A14-T6 aluminum alloy, and the composite material skin is prepared from the carbon fiber prepreg in Examples 1-6.
[0095] Comparative Example 1:
[0096] The difference from Example 6 is that the titanium dioxide / carbon nanotube composite material is replaced by multi-walled carbon nanotubes, and the multi-walled carbon nanotubes have an inner diameter of 5-10 nm, an outer diameter of 10-30 nm, and a length of 10-30 um.
[0097] Comparative Example 2:
[0098] The difference from Example 6 is that the titanium dioxide / carbon nanotube composite material is replaced by a titanium dioxide / carbon nanotube composite material prepared by another method, which specifically includes the following steps:
[0099] S1: adding tetrabutyl titanate to anhydrous ethanol while stirring the anhydrous ethanol to prepare a tetrabutyl titanate ethanol solution; the volume ratio of the anhydrous ethanol to the tetrabutyl titanate is 1:15.
[0100] S2: Mix multi-walled carbon nanotubes with anhydrous ethanol, deionized water and glacial acetic acid in a mass volume ratio of 5g:80ml:7ml:15ml to obtain a mixed liquid; then, add tetrabutyl titanate ethanol solution dropwise to the mixed liquid while stirring the mixed liquid, the dropping time is 30min, and the volume ratio of tetrabutyl titanate ethanol solution to the mixed liquid is 1:4; after the dropping is completed, continue ultrasonic treatment, the ultrasonic treatment time is 25min, the power is 800W, and a treated liquid is obtained.
[0101] The inner diameter of the multi-walled carbon nanotube is 5-10 nm, the outer diameter is 10-30 nm, and the length is 10-30 um.
[0102] S3: The treated liquid is transferred to a reactor for hydrothermal reaction at a temperature of 180°C for 12 hours. After the hydrothermal reaction, centrifugation, water washing, alcohol washing and drying are performed in sequence to obtain a titanium dioxide / carbon nanotube composite material.
[0103] Performance Testing:
[0104] The carbon fiber prepregs in Examples 1-6 and Comparative Examples 1-2 were cured and molded to prepare carbon fiber reinforced resin composite materials, and the curing system during the curing molding was 105°C / 1.5h+135°C / 3h. The prepared carbon fiber reinforced resin composite material samples were tested for 0° tensile strength using "GB / T 3354-2014 Test method for tensile properties of oriented fiber reinforced polymer matrix composite materials", 0° bending strength using "GB / T 3356-2014 Test method for bending properties of oriented fiber reinforced polymer matrix composite materials", and 0° compression strength using "GB / T 3856-2005 Test method for compression properties of unidirectional fiber reinforced plastic flat plates". The specific mechanical test results are shown in Table 1.
[0105] Table 1 Mechanical properties test results
[0106] 0° tensile strength / MPa 0° bending strength / MPa 0° compression strength / MPa Example 1 2521 1452 866 Example 2 2478 1395 819 Example 3 2559 1487 885 Example 4 2513 1432 853 Example 5 2545 1467 882 Example 6 2501 1406 832 Comparative Example 1 2383 1290 745 Comparative Example 2 2460 1368 799
[0107] As shown in Table 1, the carbon fiber reinforced resin composite material prepared from the carbon fiber prepreg obtained by the method in Examples 1-6 of the present invention has excellent mechanical properties. As shown in Comparative Example 1 compared with Example 6, the strength of the obtained carbon fiber reinforced resin composite material can be significantly improved by modifying the multi-walled carbon nanotubes by the method in the present invention. As shown in Comparative Example 2 compared with Example 6, if the multi-walled carbon nanotubes are not oxidized when they are modified, and are not subsequently calcined, the modification effect of the obtained titanium dioxide / carbon nanotube composite material will be weakened.
[0108] The above are preferred embodiments of the present invention, but the present invention is not limited to the described embodiments. It should be noted that for those skilled in the art, without departing from the principles of the present invention, changes, improvements and modifications to these embodiments should be considered as the protection scope of the present invention.
Claims
1. A carbon fiber prepreg, characterized in that: The carbon fiber prepreg comprises the following raw materials in weight percentage: 55-65% carbon fiber cloth and 35-45% epoxy resin mixture; The epoxy resin mixture comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 2.8-4.2 parts of titanium dioxide / carbon nanotube composite material, 0.01-0.05 parts of silane coupling agent, 30-35 parts of curing agent, and 0.5-1.5 parts of curing accelerator.
2. The carbon fiber prepreg according to claim 1, characterized in that The preparation method of the titanium dioxide / carbon nanotube composite material comprises the following steps: S1: adding tetrabutyl titanate to the anhydrous ethanol while stirring the anhydrous ethanol to prepare a tetrabutyl titanate ethanol solution; S2: uniformly mixing the oxidized carbon nanotubes with anhydrous ethanol, deionized water and glacial acetic acid to obtain a mixed liquid; then dropping a tetrabutyl titanate ethanol solution into the mixed liquid while stirring the mixed liquid, and after the dropping is completed, continuing ultrasonic treatment to obtain a treated liquid; S3: The treated liquid is transferred to a reactor for hydrothermal reaction. After the hydrothermal reaction is completed, centrifugation, water washing, alcohol washing, and drying are performed in sequence, and then calcination is performed under a nitrogen atmosphere to obtain a titanium dioxide / carbon nanotube composite material.
3. The carbon fiber prepreg according to claim 2, characterized in that: In step S1, the volume ratio of anhydrous ethanol to tetrabutyl titanate is 1-1.5:15-20; in step S2, the mass volume ratio of the oxidized carbon nanotubes to anhydrous ethanol, deionized water, and glacial acetic acid is 2.5-5g:60-80ml:4.5-7ml:12-15ml; The volume ratio of the tetrabutyl titanate ethanol solution in step S1 to the mixed liquid in step S2 is 1:3.5-5.
4. The carbon fiber prepreg according to claim 2, characterized in that: In step S2, the preparation method of oxidized carbon nanotubes includes the following steps: placing multi-walled carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, wherein the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution is 2-3:1; then performing ultrasonic treatment for 3-8 hours while stirring, and the power of the ultrasonic treatment is 200-300W; and then centrifuging, washing with water, and drying to obtain oxidized carbon nanotubes.
5. The carbon fiber prepreg according to claim 4, characterized in that: The multi-walled carbon nanotube has an inner diameter of 5-10 nm, an outer diameter of 10-30 nm, and a length of 10-30 um.
6. The carbon fiber prepreg according to claim 2, characterized in that: In step S2, the dripping time is 30-40 min; the ultrasonic treatment time is 20-30 min, and the ultrasonic treatment power is 500-1000W.
7. The carbon fiber prepreg according to claim 2, characterized in that: In step S3, the temperature of the hydrothermal reaction is 150-180°C and the time is 12-24h; The calcining in a nitrogen atmosphere comprises: firstly heating to 200-260° C., keeping the temperature for 0.5-1 hour, then heating to 400-430° C., keeping the temperature for 1.5-2.5 hours.
8. The carbon fiber prepreg according to claim 1, characterized in that: The epoxy resin is one or more of epoxy resin E-44 and E-51; the silane coupling agent is 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane or 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane; The curing agent is one or more of D230 and D400, and the curing accelerator is DMP-30; The carbon fiber cloth is a unidirectional carbon fiber cloth.
9. A method for preparing a carbon fiber prepreg as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S1: uniformly mixing the titanium dioxide / carbon nanotube composite material and the silane coupling agent, then adding them to the epoxy resin, heating to 65-70° C. and stirring and mixing, then adding the curing agent and the curing accelerator and stirring and mixing to obtain an epoxy resin mixture; S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 65-70°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the carbon fiber cloth, and the composite is hot-pressed by a roller at a composite temperature of 70-75°C, and then cooled to prepare a carbon fiber prepreg.
10. An application of the carbon fiber prepreg as described in any one of claims 1 to 8 or the carbon fiber prepreg prepared by the preparation method as described in claim 9 in a wing structure, the wing structure comprising an aluminum alloy skeleton and a composite material skin, the cavity between the aluminum alloy skeleton and the composite material skin is filled with foam; the composite material skin is prepared from the carbon fiber prepreg.
Citation Information
Cited By
High-strength carbon fiber plate and processing technology thereof
CN119798921A
High-strength carbon fiber plate and processing technology thereof
CN119798921B