Lignin modified PBS biodegradable plastic and preparation method thereof
Through the blending of ethyl acetate-grade lignin and PBS and the high-temperature treatment of lipoic acid, a strong interface effect is formed, which solves the problems of complex and insufficient ductility of lignin-modified PBS in the prior art, and achieves high mechanical properties and environmental protection Biodegradable plastic preparation.
Patent Information
- Application Number
- CN202411250381.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-06
AI Technical Summary
In the prior art, the lignin-modified PBS has complex processes, many additives used, high reaction toxicity and no effective improvement in ductility, and environmental protection problems.
Ethyl acetate graded lignin is blended with PBS, and lipoic acid is added at high temperature to form a strong interface effect through hydrogen bond and disulfide bond exchange, improving the compatibility and mechanical properties of lignin and PBS, simplifying the process and reducing Energy consumption.
It significantly improves the ductility, mechanical properties, ultraviolet resistance and antibacterial properties of PBS, simplifies the preparation process, reduces energy consumption and toxicity, and complies with the green sustainable development goals.
Smart Images

Figure CN118909411A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biodegradable plastics, and mainly relates to a lignin-modified PBS biodegradable plastic and a preparation method thereof. Background Art
[0002] With the rapid development of my country's economy, the consumption of disposable biodegradable plastic products on the market has increased year by year. In 2022, China's consumption of disposable biodegradable plastics reached 653,400 tons. Polybutylene succinate (PBS) is a fully biodegradable plastic synthesized from raw materials such as butanediol and succinic acid. PBS has good degradability and biocompatibility, and is widely used in food packaging, medical devices, agricultural mulch and other fields. It is an environmentally friendly plastic material. PBS itself has a large tensile strength but poor ductility. Therefore, research on improving its mechanical properties and reducing costs through filler filling is of great significance to the research on PBS.
[0003] Lignin is the second most abundant biomass resource in the world. It has abundant benzene ring structures, aliphatic and aromatic hydroxyl groups, quinone groups and other active groups, and has good biocompatibility. Industrial lignin is a by-product of the pulp and paper industry and the biorefining industry, with huge output but low utilization rate. Applying lignin in the preparation of PBS can effectively improve the mechanical properties of the composite material.
[0004] However, the prior art adopts lignin to improve the mechanical properties of PBS and often needs to modify lignin and add multiple additives to improve the compatibility of lignin and PBS. CN106700442A discloses a lignin-modified PBS biodegradable plastic and a preparation method thereof, wherein the method obtains lignin-PBS composite plastic by blending composite-modified lignin, polybutylene succinate, and functional additives in different proportions. However, the composition of this method is too complicated, a large amount of functional additives are used in the modification, and the ductility of its composite material is not high, and the elongation at break is only 360%. CN109575534A discloses a biomass reinforcing agent, a modified PBS material and a preparation method thereof, wherein the method is to assemble modified lignin and polylactide-polybutyrolactone block copolymer into a core-shell structure as a biomass reinforcing agent, and then blend it with PBS to obtain a modified PBS material, but the preparation of its reinforcing agent requires the use of ethylene glycol dimethyl ether and formaldehyde, the reaction toxicity is large and not environmentally friendly, the modification time is too long, and microwave radiation is also required, and the problem of material ductility is not paid attention to. Therefore, the basic problems existing in the current existing technologies are: the modification process is complicated and time-consuming; there are many types of components; the ductility of the material is not effectively improved and the reaction is highly toxic and not environmentally friendly. Summary of the invention
[0005] In order to solve the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a lignin-modified PBS degradable plastic.
[0006] Another object of the present invention is to provide a method for preparing lignin-modified PBS degradable plastic.
[0007] Another object of the present invention is to provide a lignin-modified PBS degradable plastic for use in the preparation of film products, medical products, packaging materials, tableware, and bio-foaming materials.
[0008] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0009] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 5 to 10 parts of ethyl acetate graded lignin.
[0010] The present invention adopts ethyl acetate fractionation to effectively homogenize lignin, and can obtain lignin with a specific structure and molecular weight. Ethyl acetate can dissolve lignin with a lower molecular weight and higher phenolic hydroxyl and methoxyl content in lignin, and can effectively reduce the polymer dispersibility index (PDI) of lignin, so that the molecular weight distribution of lignin is uniform. Polar functional groups such as phenolic hydroxyl groups with a higher content in ethyl acetate graded lignin form hydrogen bonds with PBS. Low molecular weight reduces steric hindrance and segment length in the stretching process, and is more conducive to the penetration of ethyl acetate graded lignin into the PBS molecular chain, thereby improving the effect of non-covalent bonds between ethyl acetate graded lignin and PBS. Lower weight average molecular weight is also conducive to reducing the agglomeration of lignin, improving the compatibility of lignin with PBS, and then improving the mechanical properties of PBS composite materials, especially the ductility of PBS.
[0011] Solvent fractionation is an effective method for homogenizing lignin. According to different solvent solubility parameters, low dispersibility and high reactivity lignin components can be obtained by sequential fractionation. As the molecular weight decreases, the phenolic hydroxyl and methoxyl groups in lignin gradually increase, and the aliphatic hydroxyl content gradually decreases as the molecular weight decreases.
[0012] Specifically, the method for preparing ethyl acetate fractionated lignin comprises the following steps:
[0013] The alkali lignin is mixed with ethyl acetate, filtered, and the filtrate is concentrated by rotary evaporation to obtain the ethyl acetate fractionated lignin.
[0014] More specifically, the ethyl acetate fractionated lignin has a weight average molecular weight of 880-1100 and a number average molecular weight of 530-680.
[0015] More specifically, the mass ratio of the alkali lignin to ethyl acetate is 1:7-11.
[0016] More specifically, the alkali lignin and ethyl acetate are mixed for 2 to 3 hours.
[0017] The ethyl acetate solvent collected by rotary evaporation can be recovered and reused.
[0018] Specifically, the lignin-modified PBS biodegradable plastic also includes lipoic acid.
[0019] Lipoic acid melts at high temperature and obtains linear polymer chains through disulfide bond exchange, forming strong hydrogen bond interface interactions with ethyl acetate graded lignin and PBS matrix, promoting interface fusion, improving interface compatibility, and further improving the mechanical properties of the composite material.
[0020] More specifically, the lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 5 to 10 parts of ethyl acetate-graded lignin, and 1 to 5 parts of thioctic acid.
[0021] More specifically, the lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 1 to 5 parts of lipoic acid.
[0022] Preferably, the lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 3 to 4 parts of thioctic acid.
[0023] Too little lipoic acid may not be enough to form an effective reinforcement structure, but may interfere with the interaction between lignin and PBS, resulting in a decrease in mechanical properties. As the mass of lipoic acid increases, ethyl acetate-fractionated lignin and lipoic acid form a synergistic effect to jointly improve the mechanical properties of PBS plastics.
[0024] A method for preparing the lignin-modified PBS biodegradable plastic comprises the following steps:
[0025] The PBS and ethyl acetate graded lignin are mixed to obtain the lignin modified PBS biodegradable plastic.
[0026] Specifically, the preparation method of lignin-modified PBS biodegradable plastic comprises the following steps:
[0027] PBS, ethyl acetate fractionated lignin and lipoic acid are mixed to obtain PBS biodegradable plastic modified with lignin and lipoic acid.
[0028] Specifically, the mixing temperature is 130° C. to 150° C., the mixing time is 20 to 40 min, and the mixing speed is 70 to 100 rpm.
[0029] Too high a mixing temperature or too long a mixing time will deteriorate the performance of PBS.
[0030] An appropriate rotation speed will make lignin and lipoic acid more evenly dispersed in PBS, while a too high rotation speed will reduce the tensile properties of the composite material.
[0031] The invention discloses an application of lignin-modified PBS degradable plastic in the preparation of film products, medical products, packaging materials, tableware and bio-foaming materials.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] In the present invention, hydrogen bonds are formed between the polar functional groups of the ethyl acetate-graded lignin and PBS, and the low molecular weight reduces the steric hindrance and the length of the chain segments during the stretching process, reduces the agglomeration of the lignin, improves the compatibility of the lignin and PBS, thereby improving the mechanical properties of the PBS composite material and greatly improving the ductility of the PBS.
[0034] The lignin-modified PBS degradable plastic provided by the present invention has good mechanical properties, UV resistance, antibacterial properties, photothermal conversion properties and photothermal antibacterial properties.
[0035] The preparation method of the lignin-modified PBS degradable plastic of the present invention is simple, low in energy consumption, low in toxicity, and the solvent is recyclable, which saves resources and energy to a certain extent and responds to the goal of green sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The stress-strain diagrams of the PBS plastics obtained in the examples of the present invention and the comparative examples are shown in FIG.
[0037] Figure 2 The stress-strain diagrams of the PBS plastics obtained in Example 6 of the present invention and Comparative Example 1 before and after thermal aging at 60°C.
[0038] Figure 3 The stress-strain diagrams of the PBS plastics obtained in Example 6 of the present invention and Comparative Example 1 before and after ultraviolet irradiation are shown.
[0039] Figure 4 These are the photothermal effect diagrams of Example 2, Example 3, Example 6 and Comparative Example 1 of the present invention.
[0040] Figure 5 The UV transmittance diagrams of Example 2, Example 6, Comparative Example 1 and Comparative Example 5 of the present invention are shown.
[0041] Figure 6 The antibacterial and photothermal antibacterial images of Example 2, Example 6, Comparative Example 1 and Comparative Example 5 of the present invention are shown in FIG. DETAILED DESCRIPTION
[0042] The following examples further illustrate the bioplastic film of the present invention, its preparation method and application. The examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples. The experimental methods in the following examples, unless otherwise specified, are conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, were purchased from conventional biochemical reagent stores.
[0043] The preparation method of ethyl acetate fractionated lignin in the embodiment of the present invention and comparative example 3 comprises the following steps:
[0044] Industrial alkali lignin (sourced from Shandong Sun Paper Co., Ltd.) was dissolved in ethyl acetate solvent and stirred at room temperature for 2.5 hours, wherein the mass ratio of industrial alkali lignin to ethyl acetate solvent was 1:9; the mixed solution was filtered, and the filtrate was concentrated and dried by rotary evaporation at 40°C to obtain ethyl acetate graded lignin.
[0045] The weight average molecular weight of the prepared ethyl acetate fractionated lignin is 880, and the number average molecular weight is 530.
[0046] Example 1
[0047] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS (manufacturer: Xinjiang Blue Mountain Tunhe Technology Co., Ltd., brand: TH803S) and 5 parts of ethyl acetate graded lignin.
[0048] The preparation method of the lignin-modified PBS biodegradable plastic comprises the following steps:
[0049] Turn on the heating device and rotating device of the open mill, set the heating temperature to 135°C, the roller speed to 90rpm, and melt PBS. Pour the ethyl acetate graded lignin on the molten PBS in small amounts and multiple times, mix it with a scraper for 10 minutes, turn off the heating device, keep the speed at 90rpm at room temperature, slowly cool it, and then remove it from the roller. Spread the obtained composite material on a dumbbell-shaped mold, melt it at 135°C for 5 minutes through a flat hot pressing machine, then pressurize it to 20MPa, turn off the heating device after melting for 10 minutes, turn on the circulating water pump to cool it, and then demold it.
[0050] Example 2
[0051] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 7.5 parts of ethyl acetate-graded lignin.
[0052] The preparation steps are the same as those in Example 1.
[0053] Example 3
[0054] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 10 parts of ethyl acetate graded lignin.
[0055] The preparation steps are the same as those in Example 1.
[0056] Example 4
[0057] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 1 part of thioctic acid.
[0058] The preparation steps are the same as those in Example 1.
[0059] Example 5
[0060] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 2 parts of thioctic acid.
[0061] The preparation steps are the same as those in Example 1.
[0062] Example 6
[0063] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 3 parts of thioctic acid.
[0064] The preparation steps are the same as those in Example 1.
[0065] Example 7
[0066] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 4 parts of thioctic acid.
[0067] The preparation steps are the same as those in Example 1.
[0068] Example 8
[0069] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 5 parts of thioctic acid.
[0070] The preparation steps are the same as those in Example 1.
[0071] Comparative Example 1
[0072] A PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS.
[0073] The preparation steps are the same as those in Example 1.
[0074] Comparative Example 2
[0075] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 7.5 parts of unfractionated lignin.
[0076] The preparation steps are the same as those in Example 1.
[0077] Comparative Example 3
[0078] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 5 parts of epoxidized soybean oil.
[0079] The preparation steps are the same as those in Example 1.
[0080] Comparative Example 4
[0081] The preparation method of ethanol fractionated lignin in this comparative example comprises the following steps:
[0082] Industrial alkali lignin (sourced from Shandong Sun Paper Co., Ltd.) was dissolved in ethanol solvent and stirred at room temperature for 2.5 hours, wherein the mass ratio of industrial alkali lignin to ethanol solvent was 1:9; the mixed solution was filtered, and the filtrate was concentrated and dried by rotary evaporation at 50°C to obtain ethanol graded lignin.
[0083] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 7.5 parts of ethanol-graded lignin.
[0084] The preparation steps are the same as those in Example 1.
[0085] Comparative Example 5
[0086] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 3 parts of thioctic acid.
[0087] The preparation steps are the same as those in Example 1.
[0088] Comparative Example 6
[0089] The preparation method of acetone fractionated lignin in this comparative example comprises the following steps:
[0090] Industrial alkali lignin (sourced from Shandong Sun Paper Co., Ltd.) was dissolved in acetone solvent and stirred at room temperature for 2.5 hours, wherein the mass ratio of industrial alkali lignin to acetone solvent was 1:9; the mixed solution was filtered, and the filtrate was concentrated and dried by rotary evaporation at 50°C to obtain acetone graded lignin.
[0091] A lignin-modified PBS biodegradable plastic comprises the following components in parts by mass: 100 parts of PBS and 7.5 parts of acetone-graded lignin.
[0092] The preparation steps are the same as those in Example 1.
[0093] Performance Testing
[0094] The embodiments and comparative examples need to be hot-pressed for performance testing. The hot-pressing operation can be to spread the mixed material on a mold, hot-melt it in a flat vulcanizer at 135°C for 5 minutes, then pressurize it to 20MPa for 10 minutes, and then cool it, demold it, and take it out.
[0095] Tensile performance test: The PBS plastics obtained in the examples and comparative examples were prepared into dumbbell-shaped specimens, and the tensile performance of the specimens was tested. The rising speed of the clamp was 50 mm·min -1 .
[0096] Heat aging test: The PBS plastics obtained in the examples and comparative examples were prepared into dumbbell-shaped specimens, placed in an oven at 60°C for heat aging, and then the tensile properties of the specimens were tested. The rising speed of the clamp was 50 mm·min -1 .
[0097] Anti-ultraviolet ability test: The PBS plastics obtained in the examples and comparative examples were prepared into rectangular strips with a thickness of 10 μm, and placed in an ultraviolet-visible spectrophotometer for scanning, with the scanning range set to 200-600 nm.
[0098] Antibacterial test: The PBS plastic obtained in the examples and comparative examples was prepared into a disc with a thickness of 0.8 mm and a diameter of 1 cm. 6 The Escherichia coli culture fluid and the Staphylococcus aureus culture fluid with 100 / ml were co-cultured at a constant temperature of 37°C for 24 hours, and the OD value of the culture fluid was tested by an enzyme marker to calculate the inhibition rate.
[0099] Photothermal antibacterial test: The PBS plastic obtained in the examples and comparative examples was prepared into a disc with a thickness of 0.8 mm and a diameter of 1 cm. The material was mixed with 200 μl of a 10 7 The bacterial solution of 100 μl / ml was irradiated under a near-infrared lamp for 10 min, 100 μl of the photothermal bacterial solution was aspirated and added to 900 μl of broth culture medium, the material and the culture medium were co-cultured at a constant temperature of 37°C for 24 h, the OD value of the culture medium was tested by an enzyme marker, and the inhibition rate was calculated.
[0100] The calculation formula of the antibacterial rate is:
[0101]
[0102] The tensile strength test and elongation at break test results of the embodiments and comparative examples are shown in Tables 1 and Figure 1 As shown:
[0103] Table 1 Test results of tensile strength and elongation at break of examples and comparative examples
[0104]
[0105]
[0106] From Table 1 and Figure 1 The data show that ethyl acetate graded lignin can effectively improve the ductility of PBS. The tensile strength of the composite material obtained by blending ethyl acetate lignin with PBS can reach more than 32MPa, and the elongation at break can reach more than 526%. The tensile strength of the composite material obtained by blending ethyl acetate lignin, lipoic acid and PBS is as high as 35.84MPa, and the elongation at break is as high as 1304%, which is 28 times higher than the elongation at break of pure PBS. Figure 1 The area integral of the stress-strain curve is used to calculate the toughness of the composite material. It is found that the area calculated for Comparative Example 1 is 11.41, the area for Example 2 is 165.54, and the area for Example 6 is 351.15. The toughness of Example 2 is 14.5 times higher than that of Comparative Example 1, and the toughness of Example 6 is 30.78 times higher than that of Comparative Example 1, indicating that the ethyl acetate graded lignin and thioctic acid in the present invention work synergistically to greatly improve the toughness of PBS.
[0107] Comparative Example 1 and Example 2 show that the tensile properties of PBS are greatly improved by adding the extracted lignin. Example 6 shows that after adding thioctic acid, thioctic acid polymerizes at high temperature to form polythioctic acid, which not only improves the dispersion of lignin in PBS, but also forms a strong hydrogen bond with lignin, so that a close network structure is formed between PBS, lignin and polythioctic acid, further enhancing the mechanical properties of PBS composite materials. As shown in Example 2 and Examples 4-5, when thioctic acid is added to the system of ethyl acetate graded lignin and PBS, the elongation at break decreases, but because the amount of thioctic acid is too small to form an effective reinforcement structure, it may interfere with the interaction between lignin and PBS, resulting in a decrease in mechanical properties. Therefore, it is necessary to control the mass ratio of PBS: extracted lignin: thioctic acid within the range of 100:7.5:(3-4) so that ethyl acetate graded lignin and thioctic acid will have a synergistic effect.
[0108] It can be seen from Comparative Example 4, Comparative Example 6 and Example 2 that the weight average molecular weight of ethanol-graded lignin is 3440, and the number average molecular weight is 1690; the weight average molecular weight of acetone-graded lignin is 3680, and the number average molecular weight is 1260; due to the large molecular weights of both, the elongation at break of the composite material is low, and ethanol-graded lignin and acetone-graded lignin cannot effectively improve the ductility of the PBS composite material.
[0109] Figure 2 The stress-strain diagram of the PBS plastic obtained in Example 6 and Comparative Example 1 before and after heat aging at 60°C. Figure 2 It can be seen that the mechanical properties of the modified PBS plastic after heat aging are reduced, but still maintain higher mechanical properties than those of PBS plastic, indicating that the synergistic effect of ethyl acetate fractionated lignin and lipoic acid can improve the thermal stability of PBS composites and thus increase the service life of PBS plastics.
[0110] Figure 3 The stress-strain diagram of the PBS plastic obtained in Example 6 and Comparative Example 1 before and after ultraviolet irradiation. Figure 3 It can be seen that the mechanical properties of the modified PBS plastic after UV irradiation are reduced, but still maintain higher mechanical properties than PBS plastic, indicating that the synergistic effect of ethyl acetate fractionated lignin and lipoic acid can improve the UV resistance of PBS composite materials.
[0111] Figure 4 1 is a photothermal effect diagram of Example 2, Example 3, Example 6 and Comparative Example 1. Figure 4 It can be seen that the addition of ethyl acetate-fractionated lignin gives the modified PBS material the ability to convert light into heat, which can convert near-infrared light irradiation to generate heat and achieve a sterilization effect.
[0112] Figure 5 2 and 6 are UV transmittance diagrams of Example 2 and Example 6 and Comparative Example 1 and Comparative Example 5. Figure 5 It can be seen that the PBS plastic modified by ethyl acetate fractionated lignin provided by the present invention has good ultraviolet shielding ability, indicating that it has excellent anti-ultraviolet performance.
[0113] Figure 6 The antibacterial and photothermal antibacterial graphs of Example 2, Example 6, Comparative Example 1 and Comparative Example 5 are shown. Figure 6 It can be seen that the modified PBS plastic provided by the present invention has a good antibacterial effect on Escherichia coli and Staphylococcus aureus. Lignin can destroy the cell wall structure and cell membrane structure of bacteria to destroy bacteria, and lipoic acid as a powerful antioxidant can remove free radicals, reduce oxidative stress and inhibit bacterial reproduction. The photothermal effect of lignin can increase the temperature of the material and effectively kill bacteria, thereby achieving an antibacterial effect.
[0114] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A lignin-modified PBS biodegradable plastic, characterized in that: The invention comprises the following components in parts by weight: 100 parts of PBS and 5 to 10 parts of ethyl acetate graded lignin.
2. The lignin-modified PBS biodegradable plastic according to claim 1, characterized in that: The preparation method of the ethyl acetate fractionated lignin comprises the following steps: The alkali lignin is mixed with ethyl acetate, filtered, and the filtrate is concentrated by rotary evaporation to obtain the ethyl acetate fractionated lignin.
3. The lignin-modified PBS biodegradable plastic according to claim 2, characterized in that: The mass ratio of the alkali lignin to ethyl acetate is 1:7-11.
4. The lignin-modified PBS biodegradable plastic according to claim 1, characterized in that: The lignin-modified PBS biodegradable plastic also includes lipoic acid.
5. The lignin-modified PBS biodegradable plastic according to claim 4, characterized in that: The invention comprises the following components in parts by weight: 100 parts of PBS, 5 to 10 parts of ethyl acetate graded lignin, and 1 to 5 parts of thioctic acid.
6. The lignin-modified PBS biodegradable plastic according to claim 5, characterized in that: The invention comprises the following components in parts by weight: 100 parts of PBS, 7.5 parts of ethyl acetate-graded lignin, and 1 to 5 parts of thioctic acid.
7. A method for preparing the lignin-modified PBS biodegradable plastic according to any one of claims 1 to 6, characterized in that: The following steps are involved: PBS and ethyl acetate fractionated lignin are mixed to obtain the lignin-modified PBS biodegradable plastic according to any one of claims 1 to 3.
8. The method for preparing the lignin-modified PBS biodegradable plastic according to claim 7, characterized in that: The following steps are involved: PBS, ethyl acetate fractionated lignin and thioctic acid are mixed to obtain the lignin-modified PBS biodegradable plastic according to any one of claims 4 to 6.
9. The method for preparing the lignin-modified PBS biodegradable plastic according to claim 7, characterized in that: The mixing temperature is 130° C. to 150° C., the mixing time is 20 to 40 min, and the mixing speed is 70 to 100 rpm.
10. Use of the lignin-modified PBS degradable plastic according to any one of claims 1 to 6 in the preparation of film products, medical products, packaging materials, tableware, and bio-foaming materials.
Citation Information
Patent Citations
Lignin modified PBS biodegradable plastic and preparation method thereof
CN106700442A
Modified lignin / PBS bioplastic film and preparation method thereof
CN111349253A
Lignin / PBAT composite film material and preparation method and application thereof
CN114474449A
Method for preparing recoverable polyester in one step based on full-biomass-based acid-alcohol system
CN114656623A
Green and safe biodegradable material as well as preparation method and application thereof
CN116589836A