Polyarylene ether nitrile-based composite film material with high thermal conductivity and low friction coefficient as well as preparation method and application of polyarylene ether nitrile-based composite film material

Through nucleophilic substitution reaction and co-deposition surface effect, combined with modified inorganic particles, the problem of insufficient thermal conductivity and frictional properties of polyarylethernitrile composite materials is solved, and a polyarylethernitrile composite film with high thermal conductivity and low friction coefficient is achieved Material, suitable for high-performance electronic structural parts.

CN118909425APending Publication Date: 2024-11-08UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411152982.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing polyarylethernitrile composite materials are limited by low intrinsic thermal conductivity and high friction coefficient in electronic applications, and it is difficult to meet the requirements under severe friction conditions.

Method used

Using nucleophilic substitution reaction, co-deposition surface effect and modified inorganic particles, one-dimensional silicon carbide whiskers and two-dimensional boron nitride nanosheets are used as thermal fillers and reinforcers, and dopamine and polyvinylimide are combined as surfaces. Modifier improves the compatibility of hybrid fillers and matrix resins, and forms a polyarylethernitrile-based composite film material with high thermal conductivity and low friction coefficient.

Benefits of technology

It significantly improves the thermal conductivity and wear resistance of the material, reduces the friction coefficient, enhances the deformation resistance of the composite material, and is suitable for high-performance electronic structural parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909425A_ABST
    Figure CN118909425A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a polyarylene ether nitrile-based composite film material with high thermal conductivity and low friction coefficient, and belongs to the technical field of preparation of multifunctional composite materials. According to the invention, one-dimensional silicon carbide whiskers (SiCws) and two-dimensional boron nitride nanosheets (BNNS) are used as heat-conducting fillers and reinforcements, dopamine and polyethylene imide are used as surface modifiers, and polyarylene ether nitrile is used as a polymer matrix. The method comprises the following steps: firstly, preparing inorganic modified particles from polydopamine and polyethylene imide through a surface codeposition effect, and then blending the inorganic modified particles with a polyarylene ether nitrile resin solution according to different mass fraction ratios by combining a solution tape casting method to form a film. And the interfacial interaction between the filler and the polyarylene ether nitrile matrix resin can be enhanced, so that the polyarylene ether nitrile-based composite film material with high thermal conductivity and low friction coefficient is obtained, and the polyarylene ether nitrile-based composite film material has huge application potential in high-performance electronic structural parts and can be produced and applied in a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of multifunctional composite material preparation, and relates to the synthesis of polymer materials and the preparation and processing technology of nano-composite materials, and specifically relates to a method for preparing a polyarylether nitrile-based composite film material, and in particular to a method for preparing a polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient. Background Art

[0002] As a special engineering plastic, poly(arylether nitrile) (PEN) not only has heat resistance, corrosion resistance, good processability and excellent mechanical properties, but is also widely used in defense, aerospace, electronic equipment and other fields. However, its low intrinsic thermal conductivity and high friction coefficient severely limit its application in structural parts in the electronic field, and it is not enough to meet the application requirements under severe friction conditions.

[0003] At present, researchers have carried out a series of work on high thermal conductivity polyarylethernitrile composite materials and wear-resistant polyarylethernitrile composite materials, but there is no report on polyarylethernitrile-based composite film materials with both high thermal conductivity and low friction coefficient. For example, patent CN202211598334.4 discloses a method for preparing a high thermal conductivity film material by simply blending styrene and boron nitride nanosheets, in which the thermal conductive filler is filled in a large amount, and the large component of organic matter does not have a good ability to bear friction; patent CN202410157593.6 discloses a method for preparing a high thermal conductivity insulating polyarylethernitrile film material, which reduces the filling amount of the thermal conductive filler by preparing a core-shell structure, but has a weakening effect on the self-lubricating film area; patent CN202211531892.9 discloses a method for preparing a polyarylethernitrile self-lubricating multi-component composite material, which increases the wear resistance of the matrix by adding polytetrafluoroethylene and carbon fiber, but the friction performance is limited due to poor compatibility, and the high content of filling further increases the cost.

[0004] Based on this, how to obtain a polyarylethernitrile-based composite material with high thermal conductivity and low friction coefficient is a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention

[0005] In view of this, the purpose of the present invention is to address the problems existing in the background technology and propose a high thermal conductivity, low friction coefficient polyarylethernitrile-based composite film material and its preparation method and application. The present invention adopts filler modification technology to improve the compatibility with the matrix resin, which can not only reduce the interface phonon scattering, but also improve the degree of heat conduction path shape, and finally synergistically obtain the expected composite material.

[0006] It should be noted that the present invention designs a crystalline phase in an organic polymer to increase hardness, modifies inorganic particles to achieve the construction of a reinforcement phase, and simultaneously improves the compatibility between the hybrid filler and the matrix resin through the co-deposition effect. The synergistic effects of multiple parties construct a technical effect of 1+1>2, thereby providing a method for preparing a polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient and excellent comprehensive performance.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The first technical purpose of the present invention is to provide a high thermal conductivity, low friction coefficient polyarylether nitrile-based composite film material, the material is obtained by nucleophilic substitution reaction, co-deposition surface effect, design of modified inorganic particles, compatibility improvement and solution casting method, and the polymer in the high thermal conductivity, low friction coefficient polyarylether nitrile-based composite film material is polyarylether nitrile, the inorganic filler is one-dimensional silicon carbide whiskers and two-dimensional boron nitride nanosheets, and the surface deposition modifier is dopamine and polyethyleneimide.

[0009] Specifically, the present invention proposes a method of simple nucleophilic substitution reaction, co-deposition surface effect, design of modified inorganic particles, compatibility improvement and solution casting to obtain a poly(arylether nitrile)-based composite thin film material with high thermal conductivity and low friction coefficient. The present invention selects one-dimensional silicon carbide whiskers (SiCws) and two-dimensional boron nitride nanosheets (BNNS) as thermal conductive fillers and reinforcements, dopamine and polyethyleneimide as surface modifiers, and poly(arylether nitrile) as a polymer matrix. First, polydopamine and polyethyleneimide are used to prepare modified inorganic particles through surface co-deposition effect, and then the modified inorganic particles are blended with poly(arylether nitrile) resin solution in different mass fraction ratios in combination with solution casting to form a film. This method can not only effectively improve the agglomeration of fillers in the matrix resin, but also strengthen the interface interaction between fillers and poly(arylether nitrile) matrix resin, so as to obtain a poly(arylether nitrile)-based composite thin film material with high thermal conductivity and low friction coefficient, which has great application potential in high-performance electronic structural parts and can be mass-produced and applied.

[0010] The second technical purpose of the present invention is to provide a method for preparing the polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient as described above, which specifically comprises the following steps:

[0011] Step 1: Synthesis of low molecular weight hydroxyl-terminated poly(arylene ether nitrile)

[0012] 1.1 Add hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants into a three-necked flask equipped with a thermometer, a water separator, a condensation reflux device and a mechanical stirring device, add potassium carbonate as a catalyst, and obtain a mixture powder; inject 15 mL of toluene and 15 mL of water into the water separator; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.4:5:6;

[0013] 1.2 Add the mixture powder obtained in step 1.1 to a mixed solvent of N-methylpyrrolidone (NMP) and toluene to obtain a mixed solution A; wherein (1 to 1.5) mL of the mixed solvent is added to every 1 g of the mixture powder, and the volume ratio of N-methylpyrrolidone (NMP) to toluene in the mixed solvent is 3:1;

[0014] 1.3 The mixed solution A obtained in step 1.2 is heated to 145°C-150°C at a heating rate of 5°C / min in an electric heating mantle, and is kept at 145°C-150°C for 2h; then the temperature is further increased to 170°C at a heating rate of 5°C / min, and is kept at 170°C for 1h; 5mL of toluene is discharged within 3-5 seconds by opening the water separator, and then the temperature is increased to 180°C-190°C at a heating rate of 10°C / min, and is kept at 180°C-190°C for 30min-60min; finally, the temperature is lowered to 150°C, and the obtained reaction solution is poured into 0.2mol / L hydrochloric acid solution, stirred, and a strip solid A is obtained;

[0015] 1.4 The strip solid A obtained in step 1.3 is soaked in a 0.2 mol / L hydrochloric acid solution for 12 hours, crushed, and then washed 3 to 5 times with boiling tap water until the solution is neutral; the washed powder is placed in a vacuum oven and dried for 12 hours, and the obtained white powder is the hydroxyl-terminated poly(arylene ether nitrile);

[0016] Step 2: Synthesis of high molecular weight phthalonitrile-terminated poly(arylene ether nitrile)

[0017] 2.1 Add hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants into a three-necked flask equipped with a thermometer, a water separator, a condensation reflux device and a mechanical stirring device, add potassium carbonate as a catalyst, and obtain a mixture powder; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.1:5:6; inject 15 mL of toluene and 15 mL of water into the water separator;

[0018] 2.2 Add the mixture powder obtained in step 2.1 to a mixed solvent of N-methylpyrrolidone (NMP) and toluene to obtain a mixed solution B; wherein (1 to 1.5) mL of the mixed solvent is added to every 1 g of the mixture powder, and the volume ratio of N-methylpyrrolidone (NMP) to toluene in the mixed solvent is 3:1;

[0019] 2.3 The mixed solution B obtained in step 2.2 is heated to 145°C-150°C at a heating rate of 5°C / min in an electric heating mantle, and isothermally reacted at 145°C-150°C for 2 hours; then the temperature is further increased to 170°C at a heating rate of 5°C / min, and isothermally reacted at 170°C for 1 hour; the water separator is opened to discharge 5 mL of toluene within 3-5 seconds, and then the temperature is increased to 180°C-190°C at a heating rate of 10°C / min, and isothermally reacted at 180°C-190°C for 30min-60min to obtain a mixed product;

[0020] 2.4 The mixed product obtained in step 2.3 is cooled to 80°C, and then potassium carbonate, 4-nitrophthalonitrile and N-methylpyrrolidone (NMP) are added thereto, and the mixture is reacted at 80°C for 4 hours to obtain a mixed solution C; wherein the molar ratio of potassium carbonate, 4-nitrophthalonitrile and hydroquinone added in step 2.1 is 0.48:0.36:1, and 1 g of the mixture powder composed of potassium carbonate and 4-nitrophthalonitrile is mixed with (10-15) ml of N-methylpyrrolidone;

[0021] 2.5 Pour the mixed solution C obtained in step 2.4 into a 0.2 mol / L hydrochloric acid solution and stir to obtain a strip solid B; then soak the strip solid B in a 0.2 mol / L hydrochloric acid solution for 12 hours, crush it, and then wash it with boiling tap water for 3 to 5 times until the solution is neutral; the washed powder is placed in a vacuum oven and dried for 12 hours to obtain a white powder, which is the phthalonitrile-terminated polyarylethernitrile;

[0022] Step 3: Synthesize modified inorganic particles

[0023] 3.1 Prepare a weakly alkaline tris(hydroxymethylaminomethane) buffer solution in a three-necked flask (specifically 0.4 g of tris(hydroxymethylaminomethane) and 160 mL of deionized water, pH = 8.5);

[0024] 3.2 Add one-dimensional silicon carbide whiskers (0.6 g) and two-dimensional boron nitride nanosheets (0.6 g) to the buffer solution prepared in 3.1, and treat them at room temperature with high power for 2 h using ultrasonic technology;

[0025] 3.3 Dissolve dopamine hydrochloride (DA, 0.6 g) in deionized water (4 mL), mix well and then drop into the inorganic particle buffer solution prepared in 3.2, and treat with high-power ultrasound at room temperature for 4 h;

[0026] 3.4 Add polyethyleneimide (PEI, 1.8 mL) dropwise into the mixed solution prepared in 3.3 and treat with high-power ultrasound at room temperature for 4 h;

[0027] 3.5 The mixed solution obtained in 3.4 is filtered, washed, centrifuged and vacuum dried (80° C., 12 h) to finally obtain modified inorganic particles;

[0028] Step 4: Preparation of high thermal conductivity and low friction coefficient PEN / SiCws-BNNS@PDA-PEI composite film material

[0029] 4.1 The low molecular weight hydroxyl-terminated polyarylether nitrile obtained in step 1 and the high molecular weight phthalonitrile-terminated polyarylether nitrile obtained in step 2 are added to N-methylpyrrolidone (NMP), and stirred at 180-200° C. for 2-4 h, preferably at 200° C. for 2 h, to obtain a polyarylether nitrile mixture hot solution D; wherein the mass ratio of the low molecular weight hydroxyl-terminated polyarylether nitrile to the high molecular weight phthalonitrile-terminated polyarylether nitrile is 1:1, and (10-15) mL of N-methylpyrrolidone is added to each 1 g of the mixed powder of the low molecular weight hydroxyl-terminated polyarylether nitrile and the high molecular weight phthalonitrile-terminated polyarylether nitrile;

[0030] 4.2 Add the modified inorganic particle powder obtained in step 3 to N-methylpyrrolidone (NMP), and obtain a mixed solution E after ultrasonic stirring (30° C., 1 h); wherein (10-15) mL of N-methylpyrrolidone is added to every 1 g of the modified inorganic particle powder;

[0031] 4.3 Add the mixed solution E in step 4.2 to the hot solution D in step 4.1, stir and react at 180-200°C for 4-6 hours, preferably at 200°C for 4 hours, and form the final mixed hot solution into a film by a casting method to obtain a PEN / SiCws-BNNS@PDA-PEI composite thin film material; wherein the heating process of the casting method is: keep warm at 80°C, 100°C, 120°C and 160°C for 1 hour respectively, and then keep warm at 200°C and 230°C for 2 hours; wherein the mass ratio of the polyarylether nitrile mixture to the modified inorganic particles is 1:(0.05~0.30).

[0032] Further, in step 1.1, the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1: (4.1-4.6): 5: 6, preferably, the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1: 4.4: 5: 6. In step 4.2, the mass ratio of polyarylethernitrile resin to SiCws-BNNS@PDA-PEI filler is 1: 0.20.

[0033] Specifically, the mechanism of action of the above-mentioned preparation of high thermal conductivity and low friction coefficient polyarylene ether nitrile-based composite film material is as follows:

[0034] Firstly, low molecular weight hydroxyl-terminated poly(arylethernitrile) (PEN-OH) and high molecular weight phthalonitrile-terminated poly(arylethernitrile) (PEN-Ph) were synthesized by nucleophilic substitution reaction. High molecular weight phthalonitrile-terminated poly(arylethernitrile) (PEN-Ph) and low molecular weight hydroxyl-terminated poly(arylethernitrile) (PEN-OH) were used as the matrix PEN resin, in which high molecular weight PEN-Ph increased the cyano site and low molecular weight PEN-OH increased the degree of crystallinity. Secondly, the modified inorganic particles were prepared by co-deposition surface effect. On the one hand, the highly cross-linked The PDA layer and BNNS can improve the compatibility and weaken the self-agglomeration of the lamellar nanofiller through non-covalent bonds (π-π action). On the other hand, the surface of the modified inorganic particles has a large number of hydroxyl groups and amino groups, which provide potential hydrogen bonding sites for reacting with poly(arylene ether nitrile), thereby effectively improving the compatibility and self-agglomeration and increasing the thermal conductivity. Finally, the modified inorganic particles are added to the poly(arylene ether nitrile) matrix resin. After the optimal formula is obtained, the synergistic effect of the hybrid filler and the improved compatibility is utilized to enhance the thermal conductivity and wear resistance of the composite material.

[0035] The third technical purpose of the present invention is to provide the application of the polyarylethernitrile-based composite film material with high thermal conductivity and low friction coefficient as described above in the field of electronic structural parts.

[0036] Specifically, the high thermal conductivity and low friction coefficient polyarylethernitrile-based composite film material is used in flexible copper-clad laminates.

[0037] It can be seen from the above technical solutions that, compared with the prior art, the high thermal conductivity and low friction coefficient polyarylether nitrile-based composite film material provided by the present invention and its preparation method and application have the following excellent effects:

[0038] The invention provides a method for preparing a poly(arylether nitrile)-based composite film material with high thermal conductivity and low friction coefficient. The method comprises the following steps: using low molecular weight hydroxyl-terminated poly(arylether nitrile) and high molecular weight phthalonitrile-terminated poly(arylether nitrile) synthesized by nucleophilic substitution reaction, blending modified inorganic particles with the poly(arylether nitrile) mixture and casting the mixture into a film, utilizing the synergistic effect of the construction and surface modification of the modified inorganic particles and the hydrogen bonding effect to enhance the thermal conductivity path of the composite material, so as to improve the thermal conductivity of the material system. Meanwhile, the constructed modified inorganic particles can not only serve as a reinforcing body and a skeleton in a resin matrix, thereby improving the strength or toughness of the composite material, avoiding mechanical damage such as fracture and cracking of the material under mechanical action, enhancing the deformation resistance of the composite material, and thus effectively reducing the wear rate of the composite material. The small size effect, volume effect, surface effect, quantum size effect and macroscopic quantum tunneling effect of the inorganic nanoparticles can also be utilized, so that the inorganic nanoparticles can form a very large interface in the matrix resin at a low content, thereby forming a special physical network structure, thereby facilitating the improvement of the friction performance of the composite material.

[0039] In summary, the present invention proposes to obtain a high thermal conductivity, low friction coefficient polyarylether nitrile-based composite film material through simple nucleophilic substitution reaction, co-deposition surface effect, modified inorganic particle filler construction, surface compatibility improvement and the like. The preparation process is simple and the effect is obvious. It has great application potential in high-performance electronic structural parts and can be mass-produced and applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0041] Figure 1 SEM images of SiCws (a), BNNS (b), and multidimensional hybrid filler SiCws-BNNS@PDA-PEI (c).

[0042] Figure 2 This is a comparison chart of thermal conductivity data of the composite film materials prepared in Examples 1 to 3 and Comparative Example 1.

[0043] Figure 3 This is a comparison chart of the friction coefficient data of the composite film materials prepared in Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION

[0044] The following will be combined with the embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] The embodiment of the invention discloses a method for preparing a polyarylethernitrile-based composite film material with high thermal conductivity and low friction coefficient.

[0046] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0047] The technical solution of the present invention will be further described below in conjunction with specific embodiments.

[0048] Example 1

[0049] A method for preparing a polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient comprises the following steps:

[0050] Step 1, synthesis of low molecular weight hydroxyl-terminated poly(arylene ether nitrile):

[0051] 1.1 Add hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants into a three-necked flask equipped with a thermometer, a water separator, a condensation reflux device and a mechanical stirring device, add potassium carbonate as a catalyst, and obtain a mixture powder; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.4:5:6; specifically, 3.3 g of hydroquinone, 24.21 g of biphenol, 25.80 g of 2,6-dichlorobenzonitrile, 26.87 g of potassium carbonate, and inject 15 mL of toluene and 15 mL of water into the water separator;

[0052] 1.2 Add the mixture powder obtained in step 1.1 to a mixed solvent of N-methylpyrrolidone (NMP) and toluene to obtain a mixed solution A; wherein 1.5 mL of the mixed solvent is added to every 1 g of the mixture powder, and the volume ratio of N-methylpyrrolidone (NMP) to toluene in the mixed solvent is 3:1; specifically, 60 mL of NMP and 20 mL of toluene;

[0053] 1.3 The mixed solution A obtained in step 1.2 was heated to 150°C at a heating rate of 5°C / min in an electric heating mantle, and reacted at 150°C for 2h; then the temperature was further increased to 170°C at a heating rate of 5°C / min, and reacted at 170°C for 1h; the water separator was opened to discharge 5mL of toluene within 3-5 seconds, and then the temperature was increased to 180°C at a heating rate of 10°C / min, and reacted at 180°C for 50min; finally, the temperature was lowered to 150°C, and the obtained reaction solution was poured into 0.2mol / L hydrochloric acid solution and stirred to obtain a strip solid A;

[0054] 1.4 The strip solid A obtained in step 1.3 is soaked in a 0.2 mol / L hydrochloric acid solution for 12 hours, crushed, and then washed 3 to 5 times with boiling tap water until the solution is neutral; the washed powder is placed in a vacuum oven and dried for 12 hours, and the obtained white powder is the hydroxyl-terminated poly(arylene ether nitrile);

[0055] Step 2, synthesis of high molecular weight phthalonitrile-terminated poly(arylene ether nitrile):

[0056] 2.1 Add hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants into a three-necked flask equipped with a thermometer, a water separator, a condensation reflux device and a mechanical stirring device, add potassium carbonate as a catalyst, and obtain a mixture powder; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.1:5:6; specifically, 3.3 g of hydroquinone, 13.53 g of biphenol, 25.80 g of 2,6-dichlorobenzonitrile, 26.87 g of potassium carbonate, and inject 15 mL of toluene and 15 mL of water into the water separator;

[0057] 2.2 Add the mixture powder obtained in step 2.1 to a mixed solvent of N-methylpyrrolidone (NMP) and toluene to obtain a mixed solution B; wherein 1.5 mL of the mixed solvent is added to every 1 g of the mixture powder, and the volume ratio of N-methylpyrrolidone (NMP) to toluene in the mixed solvent is 3:1; specifically, 60 mL of NMP and 20 mL of toluene;

[0058] 2.3 The mixed solution B obtained in step 2.2 was heated to 150°C at a heating rate of 5°C / min in an electric heating mantle, and reacted at 150°C for 2 hours; then the temperature was further increased to 170°C at a heating rate of 5°C / min, and reacted at 170°C for 1 hour; the water separator was opened to discharge 5 mL of toluene within 3 to 5 seconds, and then the temperature was increased to 180°C at a heating rate of 10°C / min, and reacted at 180°C for 30 minutes to 60 minutes to obtain a mixed product;

[0059] 2.4 The mixed product obtained in step 2.3 is cooled to 80°C, and then potassium carbonate, 4-nitrophthalonitrile and N-methylpyrrolidone (NMP) are added thereto, and the mixture is reacted at a constant temperature of 80°C for 4 hours to obtain a mixed solution C; wherein the molar ratio of potassium carbonate, 4-nitrophthalonitrile and hydroquinone added in step 2.1 is 0.48:0.36:1, specifically, 20.10 g of potassium carbonate, 18.88 g of 4-nitrophthalonitrile, and 3.3 g of hydroquinone; 1 g of the mixture powder composed of potassium carbonate and 4-nitrophthalonitrile is mixed with 15 ml of N-methylpyrrolidone;

[0060] 2.5 Pour the mixed solution C obtained in step 2.4 into a 0.2 mol / L hydrochloric acid solution and stir to obtain a strip solid B; then soak the strip solid B in a 0.2 mol / L hydrochloric acid solution for 12 hours, crush it, and then wash it with boiling tap water for 3 to 5 times until the solution is neutral; the washed powder is placed in a vacuum oven and dried for 12 hours to obtain a white powder, which is the phthalonitrile-terminated polyarylethernitrile;

[0061] Step 3: Synthesis of multidimensional hybrid filler SiCws-BNNS@PDA-PEI:

[0062] 3.1 Prepare a weakly alkaline tris(hydroxymethylaminomethane) buffer solution in a three-necked flask (specifically 0.4 g of tris(hydroxymethylaminomethane) and 160 mL of deionized water, pH = 8.5);

[0063] 3.2 Add one-dimensional silicon carbide whiskers (0.6 g) and two-dimensional boron nitride nanosheets (0.6 g) to the buffer solution prepared in 3.1, and treat them at room temperature with high power for 2 h using ultrasonic technology;

[0064] 3.3 Dissolve dopamine hydrochloride (DA, 0.6 g) in deionized water (4 mL), mix well and then drop into the inorganic particle buffer solution prepared in 3.2, and treat with high-power ultrasound at room temperature for 4 h;

[0065] 3.4 Add polyethyleneimide (PEI, 1.8 mL) dropwise into the mixed solution prepared in 3.3 and treat with high-power ultrasound at room temperature for 4 h;

[0066] 3.5 The mixed solution obtained in 3.4 was filtered, washed, centrifuged, and vacuum dried (80°C, 12h) to finally obtain SiCws-BNNS@PDA-PEI filler with a multi-dimensional hybrid structure;

[0067] Step 4: Preparation of poly(arylether nitrile) / multidimensional hybrid filler composite film material

[0068] 4.1 The low molecular weight hydroxyl-terminated polyarylether nitrile obtained in step 1 and the high molecular weight phthalonitrile-terminated polyarylether nitrile obtained in step 2 are added to N-methylpyrrolidone (NMP), and stirred at 200°C for 2h to obtain a hot solution D of a polyarylether nitrile mixture; wherein the mass of the low molecular weight hydroxyl-terminated polyarylether nitrile is 1g, the mass of the high molecular weight phthalonitrile-terminated polyarylether nitrile is 1g, and the amount of the solvent of N-methylpyrrolidone is 20mL;

[0069] 4.2 The multidimensional hybrid filler powder obtained in step 3 is added to N-methylpyrrolidone (NMP), and then ultrasonicated at 30° C. for 1 h to obtain a mixed solution E; wherein the mass of the multidimensional hybrid filler is 0.4 g, and the amount of the solvent N-methylpyrrolidone is 2 mL;

[0070] 4.3 Add the mixed solution E in step 4.2 to the mixed hot solution D in step 4.1, keep stirring and reacting at 200°C for 4 hours, and form the final mixed hot solution into a film by a casting method to obtain a PEN / SiCws-BNNS@PDA-PEI composite thin film material; wherein, the heating process of the casting method film formation is: keep warm at 80°C, 100°C, 120°C and 160°C for 1 hour respectively, and then keep warm at 200°C and 230°C for 2 hours; wherein the mass ratio of the polyarylethernitrile mixture to the multidimensional hybrid filler is 1:0.2, specifically, for every 2g of polyarylethernitrile, 0.4g of multidimensional hybrid filler is filled.

[0071] The properties of the PEN / SiCws-BNNS@PDA-PEI-20wt% composite film material obtained in Example 1 are as follows: thermal conductivity is 2.585 W / m·K, and friction coefficient is 0.176.

[0072] Example 2

[0073] Compared with Example 1, this embodiment is different in that: a modification is made in step 3:

[0074] Step 3: Synthesis of one-dimensional SiCws@PDA-PEI modified filler:

[0075] 3.1 Prepare a weakly alkaline tris(hydroxymethylaminomethane) buffer solution in a three-necked flask (specifically, 0.4 g of tris(hydroxymethylaminomethane) and 160 mL of deionized water, pH = 8.5);

[0076] 3.2 Add one-dimensional silicon carbide whiskers (0.6 g) to the buffer solution prepared in 3.1 and treat at room temperature with high power for 2 h using ultrasonic technology;

[0077] 3.3 Dissolve dopamine hydrochloride (DA, 0.6 g) in deionized water (4 mL), mix well and then drop into the inorganic particle buffer solution prepared in 3.2, and treat with high-power ultrasound at room temperature for 4 h;

[0078] 3.4 Add polyethyleneimide (PEI, 1.8 mL) dropwise into the mixed solution prepared in 3.3 and treat with high-power ultrasound at room temperature for 4 h;

[0079] 3.5 The mixed solution obtained in 3.4 was filtered, washed, centrifuged and vacuum dried (80°C, 12h) to finally obtain a one-dimensional SiCws@PDA-PEI filler with a rough surface;

[0080] Step 4: Preparation of poly(arylene ether nitrile) / one-dimensional silicon carbide whisker filler composite film

[0081] 4.1 The low molecular weight hydroxyl-terminated polyarylether nitrile obtained in step 1 and the high molecular weight phthalonitrile-terminated polyarylether nitrile obtained in step 2 are added to N-methylpyrrolidone (NMP), and stirred at 200°C for 2h to obtain a hot solution D of a polyarylether nitrile mixture; wherein the mass of the low molecular weight hydroxyl-terminated polyarylether nitrile is 1g, the mass of the high molecular weight phthalonitrile-terminated polyarylether nitrile is 1g, and the amount of the solvent of N-methylpyrrolidone is 20mL;

[0082] 4.2 The one-dimensional modified silicon carbide whisker filler powder obtained in step 3 is added to N-methylpyrrolidone (NMP), and then ultrasonicated at 30° C. for 1 h to obtain a mixed solution E; wherein the mass of the one-dimensional modified silicon carbide whisker filler is 0.4 g, and the amount of the solvent N-methylpyrrolidone is 2 mL;

[0083] 4.3 Add the mixed solution E in step 4.2 to the hot solution D in step 4.1, keep stirring and reacting at 200°C for 4 hours, and form the final mixed hot solution into a film by a casting method to obtain a PEN / SiCws@PDA-PEI composite thin film material; wherein, the heating process of the casting method film formation is: keep warm at 80°C, 100°C, 120°C and 160°C for 1 hour respectively, and then keep warm at 200°C and 230°C for 2 hours; wherein the mass ratio of the polyarylethernitrile mixture to the one-dimensional modified silicon carbide whisker filler is 1:0.2, specifically, for every 2g of polyarylethernitrile, 0.4g of the modified one-dimensional silicon carbide whisker is filled.

[0084] The properties of the PEN / SiCws@PDA-PEI-20wt% composite film material obtained in Example 2 are as follows: thermal conductivity is 1.769 W / m·K, and friction coefficient is 0.216.

[0085] Example 3

[0086] Compared with Example 1, this embodiment is different in that: a modification is made in step 3:

[0087] Step 3: Synthesis of two-dimensional BNNS@PDA-PEI modified filler:

[0088] 3.1 Prepare a weakly alkaline tris(hydroxymethylaminomethane) buffer solution in a three-necked flask (specifically 0.4 g of tris(hydroxymethylaminomethane) and 160 mL of deionized water, pH = 8.5);

[0089] 3.2 Add the two-dimensional boron nitride nanosheets (0.6 g) to the buffer solution prepared in 3.1 and treat at room temperature with high power for 2 h using ultrasonic technology;

[0090] 3.3 Dissolve dopamine hydrochloride (DA, 0.6 g) in deionized water (4 mL), mix well and then drop into the inorganic particle buffer solution prepared in 3.2, and treat with high-power ultrasound at room temperature for 4 h;

[0091] 3.4 Add polyethyleneimide (PEI, 1.8 mL) dropwise into the mixed solution prepared in 3.3 and treat with high-power ultrasound at room temperature for 4 h;

[0092] 3.5 The mixed solution obtained in 3.4 was filtered, washed, centrifuged and vacuum dried (80°C, 12h) to finally obtain a one-dimensional BNNS@PDA-PEI filler with a rough surface;

[0093] Step 4: Preparation of poly(arylether nitrile) / two-dimensional boron nitride nanosheet filler composite film material

[0094] 4.1 The low molecular weight hydroxyl-terminated polyarylether nitrile obtained in step 1 and the high molecular weight phthalonitrile-terminated polyarylether nitrile obtained in step 2 are added to N-methylpyrrolidone (NMP), and stirred at 200°C for 2h to obtain a hot solution D of a polyarylether nitrile mixture; wherein the mass of the low molecular weight hydroxyl-terminated polyarylether nitrile is 1g, the mass of the high molecular weight phthalonitrile-terminated polyarylether nitrile is 1g, and the amount of the solvent of N-methylpyrrolidone is 20mL;

[0095] 4.2 The modified two-dimensional boron nitride nanosheet powder obtained in step 3 was added to N-methylpyrrolidone (NMP), and then ultrasonicated at 30°C for 1 hour to obtain a mixed solution E; wherein the two-dimensional BNNS@PDA-PEI filler with a rough surface was 0.4 g, and the amount of N-methylpyrrolidone solvent was 2 mL;

[0096] 4.3 Add the mixed solution E in step 4.2 to the mixed hot solution D in step 4.1, keep stirring and reacting at 200°C for 4 hours, and form the final mixed hot solution into a film by a casting method to obtain a PEN / BNNS@PDA-PEI composite thin film material; wherein, the heating process of the casting method film formation is: keep warm at 80°C, 100°C, 120°C and 160°C for 1 hour respectively, and then keep warm at 200°C and 230°C for 2 hours; wherein the mass ratio of the polyarylethernitrile mixture to the two-dimensional filler is 1:0.2, specifically, for every 2g of polyarylethernitrile, 0.4g of modified two-dimensional boron nitride nanosheets is filled.

[0097] The properties of the PEN / BNNS@PDA-PEI-20wt% composite film material obtained in Example 3 are as follows: thermal conductivity is 1.946 W / m·K, and friction coefficient is 0.238.

[0098] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples and test examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.

[0099] Comparative Example 1

[0100] Step 1, synthesis of low molecular weight hydroxyl-terminated poly(arylene ether nitrile):

[0101] 1.1 Add hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants into a three-necked flask equipped with a thermometer, a water separator, a condensation reflux device and a mechanical stirring device, add potassium carbonate as a catalyst, and obtain a mixture powder; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.4:5:6; specifically, 3.3 g of hydroquinone, 24.21 g of biphenol, 25.80 g of 2,6-dichlorobenzonitrile, 26.87 g of potassium carbonate, and inject 15 mL of toluene and 15 mL of water into the water separator;

[0102] 1.2 Add the mixture powder obtained in step 1.1 to a mixed solvent of N-methylpyrrolidone (NMP) and toluene to obtain a mixed solution A; wherein 1.5 mL of the mixed solvent is added to every 1 g of the mixture powder, and the volume ratio of N-methylpyrrolidone (NMP) to toluene in the mixed solvent is 3:1; specifically, 60 mL of NMP and 20 mL of toluene;

[0103] 1.3 The mixed solution A obtained in step 1.2 was heated to 150°C at a heating rate of 5°C / min in an electric heating mantle, and reacted at 150°C for 2h; then the temperature was further increased to 170°C at a heating rate of 5°C / min, and reacted at 170°C for 1h; the water separator was opened to discharge 5mL of toluene within 3-5 seconds, and then the temperature was increased to 180°C at a heating rate of 10°C / min, and reacted at 180°C for 50min; finally, the temperature was lowered to 150°C, and the obtained reaction solution was poured into 0.2mol / L hydrochloric acid solution and stirred to obtain a strip solid A;

[0104] 1.4 The strip solid A obtained in step 1.3 is soaked in a 0.2 mol / L hydrochloric acid solution for 12 hours, crushed, and then washed 3 to 5 times with boiling tap water until the solution is neutral; the washed powder is placed in a vacuum oven and dried for 12 hours, and the obtained white powder is the hydroxyl-terminated poly(arylene ether nitrile);

[0105] Step 2, synthesis of high molecular weight phthalonitrile-terminated poly(arylene ether nitrile):

[0106] 2.1 Add hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants into a three-necked flask equipped with a thermometer, a water separator, a condensation reflux device and a mechanical stirring device, add potassium carbonate as a catalyst, and obtain a mixture powder; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.1:5:6; specifically, 3.3 g of hydroquinone, 13.53 g of biphenol, 25.80 g of 2,6-dichlorobenzonitrile, and 26.87 g of potassium carbonate; inject 15 mL of toluene and 15 mL of water into the water separator;

[0107] 2.2 Add the mixture powder obtained in step 2.1 to a mixed solvent of N-methylpyrrolidone (NMP) and toluene to obtain a mixed solution B; wherein 1.5 mL of the mixed solvent is added to every 1 g of the mixture powder, and the volume ratio of N-methylpyrrolidone (NMP) to toluene in the mixed solvent is 3:1; specifically, 60 mL of NMP and 20 mL of toluene;

[0108] 2.3 The mixed solution B obtained in step 2.2 was heated to 150°C at a heating rate of 5°C / min in an electric heating mantle, and reacted at 150°C for 2 hours; then the temperature was further increased to 170°C at a heating rate of 5°C / min, and reacted at 170°C for 1 hour; the water separator was opened to discharge 5 mL of toluene within 3 to 5 seconds, and then the temperature was increased to 180°C at a heating rate of 10°C / min, and reacted at 180°C for 30 minutes to 60 minutes to obtain a mixed product;

[0109] 2.4 The mixed product obtained in step 2.3 is cooled to 80°C, and then potassium carbonate, 4-nitrophthalonitrile and N-methylpyrrolidone (NMP) are added thereto, and the mixture is reacted at a constant temperature of 80°C for 4 hours to obtain a mixed solution C; wherein the molar ratio of potassium carbonate, 4-nitrophthalonitrile and hydroquinone added in step 2.1 is 0.48:0.36:1, specifically, 20.10 g of potassium carbonate, 18.88 g of 4-nitrophthalonitrile, and 3.3 g of hydroquinone; 1 g of the mixture powder composed of potassium carbonate and 4-nitrophthalonitrile is mixed with 15 ml of N-methylpyrrolidone;

[0110] 2.5 Pour the mixed solution C obtained in step 2.4 into a 0.2 mol / L hydrochloric acid solution and stir to obtain a strip solid B; then soak the strip solid B in a 0.2 mol / L hydrochloric acid solution for 12 hours, crush it, and then wash it with boiling tap water for 3 to 5 times until the solution is neutral; the washed powder is placed in a vacuum oven and dried for 12 hours to obtain a white powder, which is the phthalonitrile-terminated polyarylethernitrile;

[0111] 2.6 Add the hydroxyl-terminated polyarylether nitrile obtained in step 1 and the phthalonitrile-terminated polyarylether nitrile obtained in step 2 to N-methylpyrrolidone (NMP), stir and react at 200°C for 2h to obtain a hot solution D of the polyarylether nitrile mixture, and form a film of the final mixed hot solution by a casting method to obtain a polyarylether nitrile film; wherein, the mass of the hydroxyl-terminated polyarylether nitrile, the mass of the phthalonitrile-terminated polyarylether nitrile, and the solvent amount of N-methylpyrrolidone are 20mL; the heating process of the casting method film formation is: keep warm at 80°C, 100°C, 120°C and 160°C for 1h respectively, and then keep warm at 200°C and 230°C for 2h; then after the oven is naturally cooled to room temperature, the polyarylether nitrile film material is obtained.

[0112] The properties of the PEN composite film material obtained in Comparative Example 1 are as follows: thermal conductivity is 1.01 W / m·K, and friction coefficient is 0.322.

[0113] Test example:

[0114] (1) Thermal conductivity: One-dimensional silicon carbide whiskers have a large aspect ratio, and the peeled two-dimensional boron nitride nanosheets have a large specific surface area. After the surface co-deposition effect, their unique linear structure and lamellar structure are effectively combined to form a hybrid filler, which can not only effectively improve the thermal conductivity network and form a thermal path, but also effectively reduce the interfacial thermal resistance with the matrix resin, reduce the interface scattering effect, and improve the thermal conductivity efficiency; therefore, compared with Comparative Example 1, the thermal conductivity of Examples 1-3 is improved overall.

[0115] (2) Wear resistance: One-dimensional silicon carbide whiskers and two-dimensional boron nitride nanosheets have small size effect, volume effect, surface effect, quantum size effect and macroscopic quantum tunneling effect, which enable the modified inorganic particles to form a very large interface in the matrix resin and form a special physical network structure in the polyarylethernitrile matrix resin, thereby improving the friction performance of the polyarylethernitrile-based composite film material. In addition, the inorganic particles are introduced as reinforcements, which can play a skeleton role in the resin, improve the strength of the composite film material, avoid mechanical damage such as breakage and cracks under mechanical action, enhance the deformation resistance of the composite film material, and effectively reduce the friction coefficient of the composite film material.

[0116] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A high thermal conductivity, low friction coefficient polyarylether nitrile-based composite film material, characterized in that: The material uses one-dimensional silicon carbide whiskers (SiCws) and two-dimensional boron nitride nanosheets (BNNS) as thermal conductive fillers and reinforcements, dopamine and polyethyleneimide as surface modifiers, and poly(arylether nitrile) as a polymer matrix; polydopamine (PDA) and polyethyleneimide (PEI) are used to prepare modified inorganic particles through a surface co-deposition effect, and then the modified inorganic particles are mixed with a poly(arylether nitrile) resin solution at different mass fractions to form a film by combining a solution casting method.

2. A method for preparing the high thermal conductivity and low friction coefficient polyarylether nitrile-based composite film material according to claim 1, characterized in that: The method specifically comprises the following steps: 1) Synthesize polyarylethernitrile resin; 2) Synthetic modified inorganic particles; 3) preparing polyarylether nitrile-based composite film materials; The polyarylether nitrile resin synthesized in step 1) is added to N-methylpyrrolidone, and heated and stirred until dissolved to obtain a mixed solution I; the modified inorganic particles synthesized in step 2) are added to N-methylpyrrolidone, and ultrasonicated to obtain a mixed solution II; The mixed solution I and the mixed solution II are mixed and reacted, and then film-formed by a solution casting method to obtain a polyarylether nitrile / silicon carbide whisker-boron nitride nanosheet@polydopamine-polyethyleneimide composite film material, that is, the high thermal conductivity and low friction coefficient polyarylether nitrile-based composite film material.

3. The method for preparing the polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient according to claim 2, characterized in that: The ratio of the polyarylethernitrile resin, the modified inorganic particles and N-methylpyrrolidone is 1g: 0.05-0.30g: 10-15mL.

4. The method for preparing the polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient according to claim 2, characterized in that: The temperature rising process of the solution casting method is: keep warm at 80°C, 100°C, 120°C and 160°C for 1 hour respectively, and then keep warm at 200°C and 230°C for 2 hours respectively.

5. The method for preparing a polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient according to any one of claims 2 to 4, characterized in that: The specific operation of the step 1) of synthesizing the polyarylethernitrile resin is as follows: 5.1 Synthesis of low molecular weight hydroxyl-terminated poly(arylene ether nitrile) Hydroquinone, biphenol and 2,6-dichlorobenzonitrile are used as reactants, potassium carbonate is used as a catalyst, and a mixture powder is obtained; the obtained mixture powder is added to a mixed solvent of N-methylpyrrolidone and toluene, and the mixture is kept at a constant temperature of 145°C to 150°C for 2 hours, and then the temperature is raised to 170°C for a constant temperature reaction for 1 hour; the temperature is then raised to 180°C to 190°C for a constant temperature reaction for 30 minutes to 60 minutes; finally, the temperature is lowered to 150°C, and the obtained reaction solution is poured into a hydrochloric acid solution, and stirred to obtain a strip-shaped solid A; The strip solid A is soaked in a hydrochloric acid solution, crushed, and then washed until the solution is neutral; and then dried to obtain the polyarylethernitrile I; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.4:5:6, and (1-1.5) mL of a mixed solvent is added to every 1 g of the mixed powder; and, in the mixed solvent, the volume ratio of N-methylpyrrolidone and toluene is 3:1; 5.2 Synthesis of high molecular weight phthalonitrile-terminated poly(arylene ether nitrile) Using hydroquinone, biphenol and 2,6-dichlorobenzonitrile as reactants and potassium carbonate as a catalyst to obtain a mixture powder; adding the obtained mixture powder to a mixed solvent of N-methylpyrrolidone and toluene, reacting at a constant temperature of 145°C to 150°C for 2 hours, then heating to 170°C for 1 hour; then heating to 180°C to 190°C for 30 minutes to 60 minutes; finally cooling the obtained mixed product to 80°C, adding potassium carbonate, 4-nitrophthalonitrile and N-methylpyrrolidone thereto, and reacting at a constant temperature of 80°C for 4 hours to obtain a mixed solution C; The mixed solution C is stirred in a hydrochloric acid solution to obtain a strip solid B; then the strip solid B is soaked in a hydrochloric acid solution, crushed, and then washed until the solution is neutral; and then dried to obtain the phthalonitrile-terminated polyarylether nitrile; wherein the molar ratio of hydroquinone, biphenol, 2,6-dichlorobenzonitrile and potassium carbonate is 1:4.1:5:6; (1-1.5) mL of a mixed solvent is added to every 1 g of the mixture powder; and, in the mixed solvent, the volume ratio of N-methylpyrrolidone to toluene is 3:1; the molar ratio of potassium carbonate, 4-nitrophthalonitrile and hydroquinone is 0.48:0.36:1, and every 1 g of the mixture powder consisting of potassium carbonate and 4-nitrophthalonitrile is mixed with (10-15) mL of N-methylpyrrolidone; The polyarylethernitrile resin is a mixture of low molecular weight hydroxyl-terminated polyarylethernitrile and high molecular weight phthalonitrile-terminated polyarylethernitrile in a mass ratio of 1:

1.

6. The method for preparing a polyarylether nitrile-based composite film material with high thermal conductivity and low friction coefficient according to any one of claims 2 to 4, characterized in that: The modified inorganic particles are synthesized in step 2. The main principle is to utilize dopamine DA to self-polymerize into polydopamine PDA under alkaline conditions and in an aerobic environment, and to cooperate with polyethyleneimide PEI to form a highly cross-linked layer, which adheres to the inorganic particles (one-dimensional silicon carbide whiskers, two-dimensional boron nitride nanosheets). The specific operation is as follows: 6.1 Prepare a tris(hydroxymethylaminomethane) buffer solution to make its pH = 8.5, add inorganic particles to the Tris buffer solution under alkaline conditions, and perform high-power ultrasonic treatment at room temperature to obtain an inorganic particle buffer solution; 6.2 Dissolve dopamine hydrochloride in deionized water, mix well and then drip into the inorganic particle buffer solution prepared in 6.1, and perform high-power ultrasonic treatment at room temperature to obtain a mixed solution; 6.3 Add polyethyleneimide PEI dropwise into the mixed solution prepared in 6.2, and perform high-power ultrasonic treatment at room temperature to obtain a mixed solution; 6.4 The mixed solution obtained in 6.3 is filtered, washed, centrifuged and dried for 12 hours to finally obtain modified inorganic particles.

7. Use of the high thermal conductivity, low friction coefficient polyarylether nitrile-based composite film material as claimed in claim 1 or the high thermal conductivity, low friction coefficient polyarylether nitrile-based composite film material prepared by the method as claimed in claim 2 in the field of electronic structural parts.

8. The use according to claim 7, characterized in that: Application of the high thermal conductivity and low friction coefficient polyarylethernitrile-based composite film material in flexible copper-clad laminates.