Long-life elastomer for bridge expansion joint as well as preparation and application methods of long-life elastomer

By using composite materials composed of amine curing agents, polydimethylsiloxanes and modified hollow glass microbeads in bridge expansion joints, the microporous structure and hydrophobicity are constructed, and the oxidation degradation and corrosion of traditional materials at high temperatures are solved. The problem of self-cleaning of materials and passive radiation cooling is achieved, improving performance stability and service life.

CN118909429APending Publication Date: 2024-11-08ZHONGLU JIAOKE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974643.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional bridge expansion joint materials are oxidatively degraded, easily corroded, poor aesthetics and insufficient strength in high temperature environments, resulting in reduced performance and high maintenance costs.

Method used

Using composite materials composed of amine-based curing agents, polydimethylsiloxanes, modified hollow glass microbeads and polyurethane prepolymers, the microporous structure is constructed through phase separation, combining hydrophobic and light reflection properties to achieve self-cleaning of the material. and passive radiation cooling.

Benefits of technology

The surface temperature of the material is reduced by 5-8°C, maintaining excellent appearance and performance stability, improving hydrophobicity and light reflective properties, extending service life and reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909429A_ABST
    Figure CN118909429A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of road and bridge expansion joint materials, in particular to a long-life elastomer for a bridge expansion joint and a preparation and application method thereof. The long-life elastomer for the bridge expansion joint is formed by mixing a component A and a component B according to the weight ratio of 20: 120-150, the component A comprises the following components in parts by weight: 10-15 parts of an amine curing agent, 5-10 parts of a polydimethylsiloxane curing agent and 1-2 parts of a catalyst, and the component B comprises the following components in parts by weight: 30-60 parts of modified hollow glass beads, 50-75 parts of a polyurethane prepolymer and 30-50 parts of polydimethylsiloxane. According to the long-life elastomer for the bridge expansion joint provided by the invention, phase separation of the material is realized by utilizing the thermodynamic incompatibility property of polyurethane and polydimethylsiloxane, and a hydrogen bond and a covalent cross-linked network of the modified hollow glass beads and a matrix material are constructed, so that the elastomer material has self-cleaning and passive radiation cooling capabilities finally; and the service life of the elastomer material in complex environments such as outdoor high-temperature and humid environments is greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road and bridge expansion joint materials, and in particular to a long-life elastomer for bridge expansion joints and a preparation and application method thereof. Background Art

[0002] Bridge expansion joints are a vital component of bridge engineering, and their performance is directly related to the safety, comfort and service life of the bridge. Although the traditional expansion joint design meets the needs of bridge expansion to a certain extent, it often has problems such as high maintenance cost, easy damage, and poor driving comfort.

[0003] In recent years, seamless expansion joints have achieved seamless expansion and contraction of bridges through innovative materials and structural designs, which not only improves the overall performance of bridges, but also greatly reduces maintenance costs and improves driving comfort. Polyurethane has attracted widespread attention due to its excellent strength and flexibility, good weather resistance and aging resistance, and can effectively extend the service life of seamless expansion joints. However, the polyurethane materials used in existing expansion joints also have the following problems: (1) During long-term use, the material will be exposed to high temperature for a long time, which will cause oxidation and degradation of the material, resulting in a decrease in the mechanical properties and durability of the expansion joint; (2) Acidic substances and impurities in rainwater will corrode the surface and internal structure of the expansion joint, causing corrosion and damage to the material. The penetration of rainwater will also cause expansion inside the expansion joint, further aggravating its damage; (3) The benzene ring in conventional polyurethane materials will form a yellow quinone structure under the action of ultraviolet rays, affecting the appearance of the material; (4) Due to insufficient material strength, it will collapse and partially break under long-term high loads.

[0004] The information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as acknowledging or suggesting in any form that the information constitutes the prior art known to those skilled in the art. Summary of the invention

[0005] The first purpose of the present invention is to provide a long-life elastomer for bridge expansion joints. By utilizing the characteristics of superhydrophobicity and passive radiation cooling and through formula design, the obtained elastomer can reduce the surface temperature of the material by 5-8°C and has a self-cleaning function, maintaining excellent appearance and performance stability during long-term use of bridge expansion joints.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions:

[0007] A long-life elastomer for bridge expansion joints, which is composed of a mixture of component A and component B in a mass ratio of 20:120-150;

[0008] Calculated by weight, component A includes the following components:

[0009] 10-15 parts of amine curing agent;

[0010] 5-10 parts of polydimethylsiloxane curing agent;

[0011] 1-2 parts of catalyst;

[0012] Component B includes the following components:

[0013] 30-60 parts of modified hollow glass microspheres;

[0014] Polyurethane prepolymer 50-75 parts;

[0015] 30-50 parts of polydimethylsiloxane;

[0016] Further, after the polydimethylsiloxane curing agent (PDMS curing agent) is mixed with polydimethylsiloxane in proportion, it is cured at room temperature to obtain solid polydimethylsiloxane. Since it contains a large number of hydrophobic segments, it gives the material basic hydrophobicity. At the same time, the polarity difference between polar polyurethane and non-polar polydimethylsiloxane leads to thermodynamically incompatible properties. Through the phase separation strategy, a polyurethane / polydimethylsiloxane containing a large number of micropores and controllable pore structure is constructed. The microporous structure can scatter light, so that the light is reflected and scattered multiple times inside the material, thereby improving the light reflection performance of the material. Although polyurethane itself is hydrophilic, the microporous structure formed by phase separation and the hydrophobic effect of PDMS jointly give the composite material good hydrophobicity. The material has good hydrophobicity and high light reflection and scattering properties.

[0017] Furthermore, by adjusting the mass ratio of polyurethane prepolymer to polydimethylsiloxane, the degree of phase separation of the two materials can be adjusted, thereby achieving controllable adjustment of the microporous structure of the material. Controlling the degree of phase separation and the size and distribution of the microporous structure is a technical difficulty. Excessive phase separation will lead to a decrease in the mechanical properties of the material, while the uneven distribution of the microporous structure will affect the overall performance of the material. The mass ratio of polyurethane prepolymer to polydimethylsiloxane is 2:1-1.5, which has good mechanical properties and hydrophobicity.

[0018] Furthermore, when the mass ratio of PDMS curing agent to PDMS is 1:5, rapid curing can be achieved at room temperature, and the curing time is 2 h at 25 °C.

[0019] Furthermore, the modified hollow glass microspheres are modified with ethyl isocyanate methacrylate, and the hollow glass microspheres with hydroxyl groups on the surface can be connected by hydrogen bonds between polyurethane segments by using the carbamate generated by the reaction of NCO groups and OH groups to construct a hydrogen bond network. At the same time, the carbon-carbon double bonds on the modified hollow glass microspheres can react with PDMS under the action of a catalyst to undergo a silylation reaction to construct a covalent cross-linking network, thereby improving the dispersion of the modified hollow glass microspheres in the elastomer and achieving in-situ enhancement of the elastomer. Hollow glass microspheres with high light reflection ability are evenly dispersed in polyurethane / polydimethylsiloxane, which significantly improves the roughness of the material surface, further improves the light reflection and light scattering properties of the material, and enhances the hydrophobicity of the material, achieving super-hydrophobicity on the material surface and higher passive radiation cooling performance.

[0020] Furthermore, the mass ratio of the modified hollow glass microspheres to the elastomer is 1-1.5:5, which ensures that the hydrogen bonds and covalent bonds cross-linking network are fully constructed while avoiding excessive addition that would cause filler aggregation and affect material properties.

[0021] Furthermore, the amine curing agent is an amino-terminated aliphatic diamine, which replaces the benzene ring with a fatty chain that is not easy to yellow compared to traditional aromatic diamines. The resulting polyurethane can maintain no obvious change in appearance during long-term outdoor use.

[0022] Furthermore, the polyurethane prepolymer is polypropylene glycol terminated with aliphatic isocyanate, and the aliphatic isocyanate is used to ensure the material's yellowing resistance. The molecular weight is 2000-3000, and the NCO content is 3.5-4wt%, which ensures the chain length of the polyurethane after curing, and has good strength and elongation at break to meet the deformation requirements of the expansion joint. The lower NCO content can avoid excessive heat release during the chain extension process, thereby achieving controllable reaction rate.

[0023] Furthermore, the mass ratio of the amine curing agent to the polyurethane prepolymer is 1:5, which is consistent with the curing rate of PDMS, and the two materials can be cured simultaneously during actual use.

[0024] Furthermore, the catalyst is a composite organic metal catalyst, including two or three of an organic tin, an organic mercury and an organic platinum catalyst. Preferably, the organic tin, organic mercury and organic platinum catalysts are prepared in a mass ratio of 2:1:1. The organic tin and organic mercury catalysts can accelerate the reaction of the amino group and the NCO group, while the organic platinum catalyst can accelerate the curing of PDMS and catalyze the hydrosilylation reaction between PDMS and the carbon-carbon double bonds on the modified hollow glass microspheres.

[0025] The second object of the present invention is to provide a method for preparing a long-life elastomer for bridge expansion joints, which has the same technical effect.

[0026] A method for preparing a long-life elastomer for a bridge expansion joint comprises the following steps:

[0027] S1, hollow glass microspheres modified with ethyl isocyanate methacrylate;

[0028] S2, adding an amine curing agent, a polydimethylsiloxane curing agent, and a catalyst into a reaction kettle according to a certain proportion, stirring and mixing at a high speed to obtain component A;

[0029] S3, adding polyurethane prepolymer, polydimethylsiloxane and modified hollow glass microspheres into a reaction kettle according to proportions, stirring and mixing at high speed to obtain component B;

[0030] Furthermore, step S1 includes the following steps:

[0031] S11: 10 g of hollow glass microspheres were dispersed in 250 mL of N, N-dimethylformamide by an ultrasonic disperser and dispersed at room temperature for 30 minutes; DMF has good solubility and helps to evenly disperse the hollow glass microspheres. The mixture was ultrasonically treated by an ultrasonic disperser. The vibration of the ultrasonic wave can break the agglomeration between the microspheres, improve the dispersion effect, and create favorable conditions for subsequent reactions.

[0032] S12: Set the nitrogen flow rate to 40m / min to purge the reactor for 10 minutes to remove the air in the reactor. The purpose of this step is mainly to remove the oxygen in the reactor to avoid affecting the subsequent chemical reactions and causing the generation of unnecessary by-products.

[0033] S13: Pour the mixed solution of hollow glass microspheres obtained in step S11 into the reactor after deoxygenation in step S12, heat to 80° C., add 30 g of ethyl isocyanate methacrylate and 150 μL of dibutyltin dilaurate, and stir at 300 r / min for 24 h;

[0034] Furthermore, in step S13, the hollow glass microspheres used have been activated and have active hydroxyl groups. In addition, the dibutyltin dilaurate used can specifically catalyze the addition reaction between the hydroxyl group and the isocyanate group, thereby ensuring a better grafting effect of isocyanate ethyl methacrylate on the hollow glass microspheres.

[0035] S14: The obtained mixed solution is centrifuged and completely washed with ethanol for at least three times, and dried at 60° C. to obtain modified hollow glass microspheres.

[0036] Furthermore, in step S2, the amine curing agent, the polydimethylsiloxane curing agent and the catalyst are added into the reaction kettle in proportion, the rotation speed is adjusted to 300 r / min, and stirred for 20 min until the components are evenly dispersed to obtain component A;

[0037] Furthermore, in step S3, polyurethane prepolymer, polydimethylsiloxane, and modified hollow glass microspheres are put into a reaction kettle in proportion, the rotation speed is adjusted to 500 r / min, and stirred for 30 min until they are evenly dispersed to obtain component B;

[0038] The third object of the present invention is to provide an application method of a long-life elastomer for bridge expansion joints, which has the same technical effect.

[0039] A method for applying a long-life elastomer for a bridge expansion joint comprises the following steps: when using, mixing component A and component B evenly according to a proportion, then pouring the mixture into a groove of the expansion joint, and after surface treatment, waiting for the elastomer to dry, covering it with a geotextile and curing it at room temperature for 7 days, and then removing the geotextile to obtain the long-life elastomer for the bridge expansion joint.

[0040] In summary, the present invention has the following beneficial effects:

[0041] (1) The present invention utilizes the thermodynamically incompatible properties caused by the polarity difference between polyurethane and polydimethylsiloxane to achieve phase separation of the two materials on a macroscopic level, and constructs a large number of microporous structures on a microscopic level, thereby increasing the roughness of the material surface and further enhancing the hydrophobicity of polyurethane and polydimethylsiloxane. At the same time, due to the improvement of the roughness, the large number of microporous structures improve the reflectivity of sunlight, so that the material has a certain hydrophobicity and sunlight reflectivity;

[0042] (2) The present invention introduces modified hollow glass microspheres and utilizes the high reflection and scattering capabilities of hollow glass microspheres to achieve efficient reflection of sunlight, and with the help of the high thermal conductivity of PDMS, the heat generated by solar radiation is quickly transferred to the low-temperature area, forming a macroscopic passive radiation cooling. At the same time, the hydrophobic hollow glass microspheres reduce the surface energy of the material and further increase the roughness of the material's microstructure, thereby enhancing the hydrophobicity of the material to become a super-hydrophobic material.

[0043] (3) The core of the present invention is to remove the benzene ring structure that is prone to yellowing in the traditional polyurethane structure. By adjusting the ratio of PDMS and PU, a polymer matrix with a large number of microporous structures having certain hydrophobicity and light reflection capabilities is constructed. By introducing modified hollow glass microspheres, the hydrophobicity and light reflection and scattering capabilities of the material are further improved, giving the material super hydrophobicity and self-cleaning properties, which can isolate external pollutants such as dust and water, and maintain good radiation cooling performance, making it suitable for long-term outdoor applications.

[0044] (4) In the present invention, ethyl isocyanate methacrylate is grafted onto the surface of hollow glass microspheres. The carbon-carbon double bonds on the modified hollow glass microspheres undergo a hydrosilylation reaction with PDMS under the action of a catalyst to construct a covalent cross-linked network. At the same time, the carbamate bonds can form a hydrogen bond cross-linked network with the -NH in PU. Under the action of the double cross-linked network, the modified hollow glass microspheres can be uniformly dispersed in the polymer matrix, and in-situ reinforcement of the material can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments in the records of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0046] Figure 1 This is a schematic diagram of the interaction between the internal components after the long-life elastomer for bridge expansion joints in Example 2 of the present invention is cured.

[0047] Figure 2 This is a schematic diagram of the principle of achieving passive radiation cooling and self-cleaning performance using a long-life elastomer for a bridge expansion joint in Example 2 of the present invention.

[0048] Figure numerals: 1. polydimethylsiloxane; 2. polyurethane; 3. modified hollow glass microspheres; 4. g covalent bond; 5. hydrogen bond; 6. sunlight scattering; 7. superhydrophobic interface; 8. sunlight reflection. DETAILED DESCRIPTION

[0049] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, a long-life elastomer for bridge expansion joints and its preparation and application method proposed in the present invention, its specific implementation method, characteristics and effects are described in detail as follows.

[0050] Sources of raw materials used in the embodiments and comparative examples:

[0051] Amine curing agent: hexamethylenediamine (HDA), Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0052] Polydimethylsiloxane curing agent: hydrogen-terminated polydimethylsiloxane, Zhejiang Runhe Silicone New Materials Co., Ltd.;

[0053] Polydimethylsiloxane: divinyl-terminated polydimethylsiloxane, Zhejiang Runhe Silicone New Materials Co., Ltd.;

[0054] Hollow glass microspheres: hollow glass microspheres (after activation treatment), Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0055] Polyurethane prepolymer: HDI-terminated polypropylene glycol (molecular weight 2500, NCO value 3.6wt%), BASF (China) Co., Ltd.

[0056] Ethyl isocyanate methacrylate: Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0057] Organic mercury catalyst: neomercuric phenylmercury (MG-1), Shanghai Zhengui New Materials Technology Co., Ltd.;

[0058] Organotin catalyst: stannous octoate, Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0059] Organic platinum catalyst: Karstedt Catalyst, Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0060] Conventional reagents: dibutyltin dilaurate, N,N-dimethylformamide, ethanol, etc., Sinopharm Chemical Reagent Co., Ltd.;

[0061] Experimental methods:

[0062] Aging resistance test: Referring to the standard GB / T 16422.3-2014 Plastics Laboratory Light Source Exposure Test Method Part 3 Fluorescent UV Lamp, a UV aging test for a total of 500 hours was conducted on the elastomer material using a UV aging instrument that meets the standard. The aging resistance of the material was evaluated by testing the changes in the mechanical properties and yellowing value of the material before and after the experiment.

[0063] Passive cooling performance: Use standard xenon light source and adjust the light intensity to 1.02kw·m -2 To simulate sunlight exposure, the ambient environment and the surface temperature of the material were adjusted to 25°C, and the passive cooling performance of the material was evaluated by measuring the surface temperature rise after one hour of sunlight exposure.

[0064] Example 1

[0065] The long-life elastomer for bridge expansion joints provided in this embodiment is calculated by weight, and component A includes 12 parts of hexamethylenediamine, 6 parts of hydrogen-terminated polydimethylsiloxane, 0.5 parts of neomercuric phenylmercurate, 0.25 parts of stannous octoate, and 0.25 parts of Karstedt catalyst; component B includes the following components: 60 parts of HDI-terminated polypropylene glycol, 30 parts of divinyl-terminated polydimethylsiloxane, and 40 parts of modified hollow glass microspheres.

[0066] The preparation process of a long-life elastomer for bridge expansion joints is as follows:

[0067] S1. Disperse 10g of hollow glass microspheres in 250mL of N,N-dimethylformamide by an ultrasonic disperser and disperse at room temperature for 30 minutes. Then, set the nitrogen flow rate to 40m / min to purge the reactor for 10 minutes, remove the air in the reactor, pour the hollow glass microsphere mixed solution into the reactor, heat it to 80°C, add 30g of isocyanate ethyl methacrylate and 150μL of dibutyltin dilaurate, stir at 300r / min for 24h, centrifuge the obtained mixed solution and wash it completely with ethanol at least three times, and dry it at 60°C to obtain modified hollow glass microspheres.

[0068] S2, put 12 parts of hexamethylenediamine, 6 parts of hydrogen-terminated polydimethylsiloxane, 0.5 parts of phenylmercuric neodecanoate, 0.25 parts of stannous octoate, and 0.25 parts of Karstedt catalyst into a reaction kettle, adjust the speed to 300 r / min, and stir for 20 minutes until the mixture is evenly dispersed to obtain component A;

[0069] S3, put 60 parts of HDI-terminated polypropylene glycol, 30 parts of divinyl-terminated polydimethylsiloxane, and 40 parts of modified hollow glass microspheres into a reaction kettle, adjust the speed to 500 r / min, and stir for 30 minutes until the mixture is evenly dispersed to obtain component B;

[0070] When in use, mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.

[0071] Example 2

[0072] The long-life elastomer for bridge expansion joints provided in this embodiment is calculated by weight, and component A includes 15 parts of hexamethylenediamine, 10 parts of hydrogen-terminated polydimethylsiloxane, 1 part of neomercuric phenylmercurate, 0.5 parts of stannous octoate, and 0.5 parts of Karstedt catalyst; component B includes the following components: 75 parts of HDI-terminated polypropylene glycol, 50 parts of divinyl-terminated polydimethylsiloxane, and 60 parts of modified hollow glass microspheres.

[0073] The preparation process of a long-life elastomer for bridge expansion joints is as follows:

[0074] S1. Disperse 10g of hollow glass microspheres in 250mL of N,N-dimethylformamide by an ultrasonic disperser and disperse at room temperature for 30 minutes. Then, set the nitrogen flow rate to 40m / min to purge the reactor for 10 minutes, remove the air in the reactor, pour the hollow glass microsphere mixed solution into the reactor, heat it to 80°C, add 30g of isocyanate ethyl methacrylate and 150μL of dibutyltin dilaurate, stir at 300r / min for 24h, centrifuge the obtained mixed solution and wash it completely with ethanol at least three times, and dry it at 60°C to obtain modified hollow glass microspheres.

[0075] S2, 15 parts of hexamethylenediamine, 10 parts of hydrogen-terminated polydimethylsiloxane, 1 part of phenylmercuric neodecanoate, 0.5 parts of stannous octoate, and 0.5 parts of Karstedt catalyst were added into a reaction kettle, the speed was adjusted to 300 r / min, and stirred for 20 min until the mixture was evenly dispersed to obtain component A;

[0076] S3, put 75 parts of HDI-terminated polypropylene glycol, 50 parts of divinyl-terminated polydimethylsiloxane, and 60 parts of modified hollow glass microspheres into a reaction kettle, adjust the speed to 500 r / min, and stir for 30 minutes until the mixture is evenly dispersed to obtain component B;

[0077] When in use, mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.

[0078] like Figure 1 The figure shows the interaction between the components of the long-life elastomer for bridge expansion joints after curing in Example 2. It can be found that in the cross-linked structure of polydimethylsiloxane 1 and polyurethane 2, the modified hollow glass microspheres 3 are cross-linked with polydimethylsiloxane 1 through g covalent bonds 4, and the modified hollow glass microspheres 3 are cross-linked with polyurethane 2 through hydrogen bonds 5. This shows that the present invention grafts isocyanate ethyl methacrylate onto the surface of hollow glass microspheres, and the carbon-carbon double bonds on the modified hollow glass microspheres react with PDMS under the action of a catalyst to form a covalent cross-linked network. At the same time, the carbamate bonds can form a hydrogen bond cross-linked network with -NH in the polyurethane. Under the action of the double cross-linked network, the modified hollow glass microspheres can be evenly dispersed in the polymer matrix and achieve in-situ enhancement of the material.

[0079] like Figure 2The schematic diagram of passive radiation cooling and self-cleaning performance of the long-life elastomer used in the bridge expansion joint in Example 2. The surface of the prepared long-life elastomer is a super-hydrophobic interface 7, and the hollow glass microspheres with high light reflection ability are evenly dispersed in the polyurethane / polydimethylsiloxane, which significantly improves the roughness of the material surface, further improves the sunlight reflection 8 and sunlight scattering 6 performance of the material, and enhances the hydrophobicity of the material, achieving super-hydrophobicity of the material surface and high passive radiation cooling performance.

[0080] Example 3

[0081] The long-life elastomer for bridge expansion joints provided in this embodiment is calculated by weight, and component A includes 10 parts of hexamethylenediamine, 7 parts of hydrogen-terminated polydimethylsiloxane, 0.5 parts of neomercuric phenylmercurate, 0.25 parts of stannous octoate, and 0.25 parts of Karstedt catalyst; component B includes the following components: 50 parts of HDI-terminated polypropylene glycol, 35 parts of divinyl-terminated polydimethylsiloxane, and 30 parts of modified hollow glass microspheres.

[0082] The preparation process of a long-life elastomer for bridge expansion joints is as follows:

[0083] S1. Disperse 10g of hollow glass microspheres in 250mL of N,N-dimethylformamide by an ultrasonic disperser and disperse at room temperature for 30 minutes. Then, set the nitrogen flow rate to 40m / min to purge the reactor for 10 minutes, remove the air in the reactor, pour the hollow glass microsphere mixed solution into the reactor, heat it to 80°C, add 30g of isocyanate ethyl methacrylate and 150μL of dibutyltin dilaurate, stir at 300r / min for 24h, centrifuge the obtained mixed solution and wash it completely with ethanol at least three times, and dry it at 60°C to obtain modified hollow glass microspheres.

[0084] S2, 10 parts of hexamethylenediamine, 7 parts of hydrogen-terminated polydimethylsiloxane, 0.5 parts of phenylmercuric neodecanoate, 0.25 parts of stannous octoate, and 0.25 parts of Karstedt catalyst were added into a reaction kettle, the speed was adjusted to 300 r / min, and stirred for 20 min until the mixture was evenly dispersed to obtain component A;

[0085] S3, put 50 parts of HDI-terminated polypropylene glycol, 35 parts of divinyl-terminated polydimethylsiloxane, and 30 parts of modified hollow glass microspheres into a reaction kettle, adjust the speed to 500 r / min, and stir for 30 minutes until the mixture is evenly dispersed to obtain component B;

[0086] When in use, mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.

[0087] Comparative Example 1 (Modification using ungrafted hollow glass microspheres)

[0088] The long-life elastomer for bridge expansion joints provided in this comparative example is calculated by weight as follows: Component A includes 15 parts of hexamethylenediamine, 10 parts of hydrogen-terminated polydimethylsiloxane, 1 part of neomercuric phenylmercurate, 0.5 parts of stannous octoate, and 0.5 parts of Karstedt catalyst; Component B includes the following components: 75 parts of HDI-terminated polypropylene glycol, 50 parts of divinyl-terminated polydimethylsiloxane, and 60 parts of hollow glass microspheres.

[0089] The preparation process of a long-life elastomer for bridge expansion joints is as follows:

[0090] S1, put 15 parts of hexamethylenediamine, 10 parts of hydrogen-terminated polydimethylsiloxane, 1 part of neopentylmercurate, 0.5 parts of stannous octoate, and 0.5 parts of Karstedt catalyst into a reaction kettle, adjust the speed to 300r / min, and stir for 20min until the mixture is evenly dispersed to obtain component A;

[0091] S2, put 75 parts of HDI-terminated polypropylene glycol, 50 parts of divinyl-terminated polydimethylsiloxane, and 60 parts of hollow glass microspheres into a reaction kettle, adjust the speed to 500 r / min, and stir for 30 minutes until the mixture is evenly dispersed to obtain component B;

[0092] When in use, mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.

[0093] Comparative Example 2 (Using only polyurethane without adding polydimethylsiloxane)

[0094] The long-life elastomer for bridge expansion joints provided in this comparative example is, calculated by weight, component A including 15 parts of hexamethylenediamine, 1 part of phenylmercuric neodecanoate, and 0.5 parts of stannous octoate; component B includes the following components: 75 parts of HDI-terminated polypropylene glycol and 30 parts of modified hollow glass microspheres.

[0095] The preparation process of a long-life elastomer for bridge expansion joints is as follows:

[0096] S1. Disperse 10g of hollow glass microspheres in 250mL of N,N-dimethylformamide by an ultrasonic disperser and disperse at room temperature for 30 minutes. Then, set the nitrogen flow rate to 40m / min to purge the reactor for 10 minutes, remove the air in the reactor, pour the hollow glass microsphere mixed solution into the reactor, heat it to 80°C, add 30g of isocyanate ethyl methacrylate and 150μL of dibutyltin dilaurate, stir at 300r / min for 24h, centrifuge the obtained mixed solution and wash it completely with ethanol at least three times, and dry it at 60°C to obtain modified hollow glass microspheres.

[0097] S2, add 15 parts of hexamethylenediamine, 1 part of phenylmercuric neodecanoate, and 0.5 parts of stannous octoate into a reaction kettle, adjust the speed to 300r / min, and stir for 20min until the mixture is evenly dispersed to obtain component A;

[0098] S3, put 75 parts of HDI-terminated polypropylene glycol and 30 parts of modified hollow glass microspheres into a reactor, adjust the speed to 500 r / min, and stir for 30 minutes until the mixture is evenly dispersed to obtain component B;

[0099] When in use, mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.

[0100] Comparative Example 3 (using only polydimethylsiloxane without adding polyurethane)

[0101] The long-life elastomer for bridge expansion joints provided in this comparative example is calculated by weight, and component A includes 10 parts of hydrogen-terminated polydimethylsiloxane and 0.5 parts of Karstedt catalyst; component B includes the following components: 50 parts of divinyl-terminated polydimethylsiloxane and 20 parts of modified hollow glass microspheres.

[0102] The preparation process of a long-life elastomer for bridge expansion joints is as follows:

[0103] S1. Disperse 10g of hollow glass microspheres in 250mL of N,N-dimethylformamide by an ultrasonic disperser and disperse at room temperature for 30 minutes. Then, set the nitrogen flow rate to 40m / min to purge the reactor for 10 minutes, remove the air in the reactor, pour the hollow glass microsphere mixed solution into the reactor, heat it to 80°C, add 30g of isocyanate ethyl methacrylate and 150μL of dibutyltin dilaurate, stir at 300r / min for 24h, centrifuge the obtained mixed solution and wash it completely with ethanol at least three times, and dry it at 60°C to obtain modified hollow glass microspheres.

[0104] S2, put 10 parts of hydrogen-terminated polydimethylsiloxane and 0.5 parts of Karstedt catalyst into a reaction kettle, adjust the speed to 300 r / min, and stir for 20 minutes until the mixture is evenly dispersed to obtain component A;

[0105] S3, put 50 parts of divinyl-terminated polydimethylsiloxane and 20 parts of modified hollow glass microspheres into a reaction kettle, adjust the speed to 500 r / min, and stir for 30 minutes until the mixture is evenly dispersed to obtain component B;

[0106] When in use, mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.

[0107] Performance Testing

[0108] The performance of the long-life elastomers for bridge expansion joints obtained in Examples 1-3 and Comparative Examples 1-3 was tested, and the test results are shown in Table 1.

[0109] Table 1 Performance test results of long-life elastomers for bridge expansion joints

[0110] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Water contact angle / ° 161 164 162 145 112 135 Average pore size / μm 1.6 1.4 1.3 1.4 0 0 <![CDATA[Surface temperature / °C·h -1 > 9 7 8 14 17 15 Tensile strength / MPa 13.2 13.5 13.1 8.1 10.2 6.5 Elongation at break / % 603 618 609 450 472 402 Yellowing value / Yi 2.3 2 2.2 12.2 18.3 13.1 Aging tensile strength / MPa 12.8 13.1 12.7 5.9 6.1 4.5 Aging elongation at break / % 576 595 585 389 362 289

[0111] Note: All specimens were cured at 60℃ for 3 days before testing.

[0112] It can be seen from Table 1 above that Examples 1-3 are several preferred embodiments of the present invention. It can be seen from the data that the long-life elastomer for bridge expansion joints prepared using the above materials and methods is a super hydrophobic material, the water contact angle is above 150°, the average pore size is between 1.3-1.6 μm, the surface temperature of the material is only increased by 7-9°C, and the surface temperature is reduced by about 5-10°C compared with several comparative examples. It has good mechanical properties and can meet the actual use requirements of the expansion joint. In addition, after 500 hours of UV aging test, the material has basically no yellowing and no obvious attenuation of mechanical properties, which can effectively extend the service life of the expansion joint.

[0113] Compared with Example 2, Comparative Example 1 uses ungrafted hollow glass microspheres. Since the surface of the glass microspheres cannot form hydrogen bonds and covalent bond networks with polyurethane and polydimethylsiloxane, they are unevenly dispersed in the system, and the super-hydrophobic and high solar reflective interfaces of the elastomeric materials cannot be constructed and improved. The hydrophobicity and cooling performance are also significantly reduced compared with Example 2. The mechanical properties cannot be enhanced due to the accumulation of fillers, but instead cause the mechanical properties of the elastomeric materials to be significantly attenuated. Therefore, the material has poor aging resistance, and yellowing and aging mechanical properties are reduced.

[0114] Compared with Example 2, Comparative Example 2 does not introduce non-polar polydimethylsiloxane, so phase separation does not occur, and there is no obvious pore structure on the surface of the material, which leads to a significant decrease in its hydrophobicity and a significant increase in the surface temperature. Although the mechanical properties do not decay significantly, the aging resistance of the material is significantly reduced due to the influence of hydrophobicity and surface temperature, and yellowing and material aging are the most serious.

[0115] Compared with Example 2, Comparative Example 3 did not introduce polyurethane with good mechanical properties. Similarly, no pore structure was formed because phase separation did not occur. In addition, since the mechanical properties of the polydimethylsiloxane material were much lower than those of the polyurethane material, the mechanical properties of the elastomeric material decreased significantly, and the actual use requirements of the expansion joint could not be met.

[0116] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A long-life elastomer for bridge expansion joints, characterized in that: It is composed of component A and component B mixed in a mass ratio of 20:120-150; Calculated by weight, the component A includes the following components: 10-15 parts of amine curing agent; 5-10 parts of polydimethylsiloxane curing agent; 1-2 parts of catalyst; The B component includes the following components: 30-60 parts of modified hollow glass microspheres; Polyurethane prepolymer 50-75 parts; 30-50 parts of polydimethylsiloxane; The long-life elastomer used in the bridge expansion joint has the characteristics of self-cleaning and passive radiation cooling, and can be used for a long time in complex environments such as high temperature and humidity outdoors.

2. The long-life elastomer for bridge expansion joints according to claim 1, characterized in that: The polydimethylsiloxane curing agent is hydrogen-terminated polydimethylsiloxane, and the mass ratio of the hydrogen-terminated polydimethylsiloxane to the polydimethylsiloxane is 1:

5.

3. The long-life elastomer for bridge expansion joints according to claim 1, characterized in that: The modified hollow glass microspheres are hollow glass microspheres modified with ethyl isocyanate methacrylate.

4. The long-life elastomer for bridge expansion joints according to claim 1, characterized in that: The amine curing agent is an amino-terminated aliphatic diamine.

5. The long-life elastomer for bridge expansion joints according to claim 1, characterized in that: The polyurethane prepolymer is aliphatic isocyanate-terminated polypropylene glycol with a molecular weight of 2000-3000 and an NCO content of 3.5-4wt%.

6. The long-life elastomer for bridge expansion joints according to claim 1, characterized in that: The mass ratio of the amine curing agent to the polyurethane prepolymer is 1:

5.

7. The long-life elastomer for bridge expansion joints according to claim 1, characterized in that: The catalyst is an organic metal catalyst prepared by compounding two or three of organic tin, organic mercury and organic platinum catalysts.

8. The method for preparing a long-life elastomer for bridge expansion joints according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, hollow glass microspheres modified with ethyl isocyanate methacrylate; S2, adding an amine curing agent, a polydimethylsiloxane curing agent, and a catalyst into a reaction kettle according to a certain proportion, stirring and mixing at a high speed to obtain component A; S3. Put the polyurethane prepolymer, polydimethylsiloxane and modified hollow glass microspheres into a reaction kettle in proportion, stir and mix at high speed to obtain component B.

9. The method for preparing a long-life elastomer for bridge expansion joints according to claim 8, characterized in that: Step S1 includes the following steps: S11: dispersing the hollow glass microspheres in N,N-dimethylformamide by an ultrasonic disperser; S12: Purge the reactor until oxygen in the reactor is removed; S13: pouring the hollow glass microsphere mixed solution obtained in step S11 into the reactor after deoxygenation in step S12, heating to 80° C., adding ethyl isocyanate methacrylate and dibutyltin dilaurate, and stirring to react; S14: The obtained mixed solution is centrifuged, washed and dried to obtain modified hollow glass microspheres.

10. The application method of the long-life elastomer for bridge expansion joints according to any one of claims 1 to 7, characterized in that: The following steps are involved: Mix component A and component B evenly in proportion, then pour them into the expansion joint pit. After the surface treatment, wait for the elastomer to be finger-dry, cover it with geotextile and maintain at room temperature for 7 days, then remove the geotextile to obtain the long-life elastomer for bridge expansion joints.