High-thermal-conductivity organic silicon gel and preparation method thereof
By using dopamine oxidation polymerization reaction under alkaline conditions and other technologies in thermally conductive silicone gels, an efficient thermal conductivity network is formed, which solves the problem of poor compatibility between thermal fillers and substrates, and improves thermal conductivity and stability , enhances the heat resistance and breakdown strength of the material.
Patent Information
- Application Number
- CN202410996672.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The compatibility between the thermal filler and the matrix in traditional thermally conductive silicone gels is poor, resulting in a smaller proportion of fillers, limiting the thermal conductivity. After the filling amount increases, the viscosity of the gel system increases rapidly and loses fluidity, resulting in pores after curing. and other defects, reducing the thermal conductivity of the material.
Polydopamine modified alumina is formed by dopamine oxidation polymerization under alkaline conditions, combining thiolated boron nitride with vinyl epoxy silicone and POSS to form an efficient thermal conductivity network, improving the dispersion and stability of thermal fillers, and The combination of vinyl silicone oil and branched silicone oil can improve the bonding of filler and matrix.
It significantly improves the thermal conductivity and the overall stability of the material, enhances the wrapping and fixation of the thermal filler, reduces pore defects, and improves the heat resistance and breakdown strength of the material.
Smart Images

Figure BDA0004960427590000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicone gel, in particular to a high thermal conductivity organic silicone gel and a preparation method thereof. Background Art
[0002] With the continuous development of electronic devices, the power density of electronic devices is getting higher and higher, and the requirements for their heat dissipation performance are also getting higher and higher. In order to improve the heat dissipation effect, some traditional heat dissipation materials (such as metal plates) can no longer meet the needs. Therefore, thermal conductive silicone gel as a new type of heat dissipation material has gradually attracted people's attention.
[0003] Thermally conductive silicone gel is a polymer network structure generated by cross-linking with a cross-linking agent and other additives under the action of a catalyst, and is compounded with a thermally conductive filler during the reaction, binding the thermally conductive filler in the polymer network chain to form a uniform and stable composite. The thermal conductivity of thermally conductive silicone gel is determined by the synergistic effect between the thermally conductive filler and the polysiloxane (PDMS) chain; among them, the thermally conductive filler is the main thermal conductive carrier, and the number and performance of the thermally conductive network chain formed in the PDMS matrix play a decisive role in the thermal conductivity. However, the compatibility between traditional thermally conductive fillers and the matrix is poor, resulting in a small proportion of fillers in the thermally conductive gel, which limits the thermal conductivity. With the increase in the amount of thermally conductive filler filling, the viscosity of the gel system will increase rapidly, and even lose fluidity, resulting in defects such as pores after curing, thereby significantly reducing the thermal conductivity of the material.
[0004] Therefore, we propose a high thermal conductive silicone gel and a preparation method thereof. Summary of the invention
[0005] The object of the present invention is to provide a high thermal conductivity silicone gel and a preparation method thereof to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a high thermal conductive silicone gel comprises the following steps:
[0008] Step S1: uniformly mixing the vinyl silicone oil and the composite to obtain a base rubber; the composite is compounded by polydopamine-modified alumina and epoxide boron nitride;
[0009] Step S2: uniformly mixing the base rubber, vinyl-terminated phenyl silicone oil, monovinyl-terminated methyl silicone oil, inhibitor and platinum catalyst to obtain material A;
[0010] Step S3: uniformly mixing the base rubber, monovinyl-terminated methyl silicone oil and hydrogen-containing silicone oil to obtain material B;
[0011] Step S4: Mix material A and material B evenly, and perform vacuum degassing to obtain a high thermal conductive silicone gel.
[0012] Furthermore, in step S1, the base glue includes the following components by weight: 100-110 parts of vinyl silicone oil and 300-900 parts of the composite.
[0013] Furthermore, the vinyl silicone oil is composed of linear vinyl silicone oil and branched vinyl silicone oil in a mass ratio of 1:1.
[0014] Furthermore, the viscosity of the linear vinyl silicone oil and the branched vinyl silicone oil is 90 mPa·S (25° C.).
[0015] Furthermore, the preparation method of the composite is as follows:
[0016] Step (1): adjusting the pH of the Tris-HCl buffer solution to 8.5, adding dopamine hydrochloride and mixing evenly to obtain a dopamine solution; adding alumina to the dopamine solution and stirring for 22-24 hours, filtering, washing, and drying to obtain polydopamine-modified alumina;
[0017] Step (2): evenly mix the boron nitride and the sodium hydroxide solution, stir at 70-80° C. for 10-12 hours, heat to 110-120° C. for reaction for 10-12 hours, cool to room temperature, wash, filter, and dry to obtain hydroxylated boron nitride; evenly mix the hydroxylated boron nitride, mercaptopropyltrimethoxysilane, deionized water, and anhydrous ethanol, adjust the system pH to 4-6, react at 65-75° C. for 5-7 hours, filter, wash, and dry to obtain thiolated boron nitride;
[0018] Step (3): uniformly mixing the mercapto boron nitride, vinyl epoxy silicone and octavinyl POSS, adding a photoinitiator, and irradiating with ultraviolet light to obtain epoxide boron nitride;
[0019] Step (4): uniformly mix polydopamine-modified alumina, epoxide boron nitride and anhydrous ethanol, and react at 50-60° C. for 4-6 hours to obtain a composite.
[0020] Furthermore, in step (1), the concentration of the Tris-HCl buffer is 0.01 mol / L, the concentration of the dopamine solution is 3-5 g / L, and the mass of the aluminum oxide is 10-20% of the mass of the dopamine solution.
[0021] Furthermore, in the step (2), the mass ratio of boron nitride to sodium hydroxide solution is 1:(4-5), the concentration of sodium hydroxide solution is 5-10 mol / L, and the mass ratio of hydroxylated boron nitride, mercaptopropyltrimethoxysilane, deionized water and anhydrous ethanol is 1:(0.1-0.3):(2-4):(10-15).
[0022] Furthermore, in step (3), the preparation method of vinyl epoxy silicone is as follows:
[0023] Mix 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, dimethyldimethoxysilane, anhydrous ethanol and deionized water evenly, heat to 70-80°C, add dibutyltin dilaurate, react for 3-5h, then add vinyldimethylethoxysilane, capping reaction for 2-4h, and obtain vinyl epoxy silicone by vacuum rotary evaporation.
[0024] Furthermore, the mass ratio of the 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, dimethyldimethoxysilane, anhydrous ethanol and deionized water is 1:(1.1-1.2):(5-10):(2-4).
[0025] Furthermore, the mass of the dibutyltin dilaurate is 1-3% of the mass of 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, and the mass of vinyldimethylethoxysilane is 1.2-1.4 times the mass of 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane.
[0026] Furthermore, in the step (3), the mass ratio of mercapto boron nitride, vinyl epoxy silicone, octavinyl POSS and photoinitiator is 1: (0.5-0.8): (0.3-0.5): (0.1-0.3).
[0027] Furthermore, the photoinitiator is 2-hydroxy-2-methylpropiophenone.
[0028] Furthermore, the process conditions of the ultraviolet irradiation are: irradiation wavelength 360-400nm, irradiation time 0.5-2.0h, irradiation intensity 20-35mW / cm 2 .
[0029] Furthermore, in the step (4), the mass ratio of polydopamine-modified alumina, epoxide boron nitride and anhydrous ethanol is 1:(0.5-1.0):(5-10).
[0030] Furthermore, in step S2, material A includes the following components by weight: 100-110 parts of base rubber, 3-5 parts of vinyl-terminated phenyl silicone oil, 2-4 parts of monovinyl-terminated methyl silicone oil, 1-3 parts of inhibitor, and 1-3 parts of platinum catalyst.
[0031] Furthermore, in step S3, material B includes the following components by weight: 100-110 parts of base rubber, 2-4 parts of monovinyl-terminated methyl silicone oil, and 6-12 parts of hydrogen-containing silicone oil.
[0032] Furthermore, the viscosity of the monovinyl-terminated methyl silicone oil is 2000 mPa·s (25° C.), and the mass fraction of vinyl is 0.16%.
[0033] Further, the preparation method of the vinyl-terminated phenyl silicone oil is as follows:
[0034] Diphenyldimethoxysilane, dimethyldimethoxysilane and hydrochloric acid solution are mixed evenly, reacted at 65-75°C for 2-4h, and washed, separated and dehydrated to obtain an intermediate; under nitrogen protection, the intermediate, divinyltetramethyldisiloxane and octamethylcyclotetrasiloxane are mixed evenly, tetramethylammonium hydroxide is added, reacted at 75-80°C for 3-5h, and distilled under reduced pressure to obtain vinyl-terminated phenyl silicone oil.
[0035] Furthermore, the concentration of the hydrochloric acid solution is 37 wt %.
[0036] Furthermore, the vinyl-terminated phenyl silicone oil comprises the following components by weight: 2-4 parts of diphenyldimethoxysilane, 3-5 parts of dimethyldimethoxysilane, 0.05-0.10 parts of hydrochloric acid solution, 6-8 parts of divinyltetramethyldisiloxane, 2-4 parts of octamethylcyclotetrasiloxane, and 0.01-0.03 parts of tetramethylammonium hydroxide.
[0037] Furthermore, the inhibitor is 1-ethynyl cyclohexanol.
[0038] Furthermore, in step S4, the mass ratio of material A to material B is 1:1.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] 1. A high thermal conductivity organic silicon gel and a preparation method thereof of the present invention, wherein a polydopamine coating is formed on the surface of aluminum oxide by an oxidative polymerization reaction of dopamine under alkaline conditions to obtain polydopamine-modified aluminum oxide, wherein the polydopamine coating can form multiple interactions such as hydrogen bonds, van der Waals forces and covalent bonds, which is beneficial to the combination between aluminum oxide and the organic silicon gel matrix, and improves the dispersibility and stability of the thermal conductive filler in the matrix; the surface of hydroxylated boron nitride is modified by mercaptopropyltrimethoxysilane to obtain mercaptolated boron nitride, and vinyl and mercapto groups are used to form a plurality of interactions such as hydrogen bonds, van der Waals forces and covalent bonds, which is beneficial to the combination between aluminum oxide and the organic silicon gel matrix, and improves the dispersibility and stability of the thermal conductive filler in the matrix; The thiol-ene click chemistry reaction allows the thiolated boron nitride to react with vinyl epoxy silicone and octavinyl POSS, introducing epoxy groups, silicone groups and POSS structures, so that boron nitride forms an efficient thermal conductive network in the silicone matrix, further improving the thermal conductivity of the composite material. Finally, the amino groups on the polydopamine coating are used to undergo a ring-opening reaction with the epoxy groups of vinyl epoxy silicone, so that alumina and boron nitride form a strong bond in the composite material, thereby improving the overall stability and thermal conductivity of the thermal conductive filler.
[0041] 2. A high thermal conductivity silicone gel and a preparation method thereof of the present invention obtains a base glue by uniformly mixing vinyl silicone oil and a composite, which not only improves the dispersibility of the thermally conductive filler in the PDMS system, reduces the agglomeration of the filler in the polymer matrix, but also enhances the bonding between the filler and the polymer matrix; wherein the vinyl silicone oil is composed of straight-chain vinyl silicone oil and branched vinyl silicone oil, has lower viscosity and higher fluidity, takes into account the cross-linking density of the obtained silicone gel, plays a role in the wrapping and fixation of the thermally conductive filler, thereby enhancing the bonding force between the thermally conductive filler and PMDS, and helps to improve the thermal conductivity of the overall material.
[0042] 3. The high thermal conductivity organic silicone gel and its preparation method of the present invention can improve the heat resistance of the material by adding vinyl-terminated phenyl silicone oil and introducing a rigid benzene ring structure; at the same time, the conjugated structure of the benzene ring itself has a large electron affinity, which enables it to capture high-energy electrons and dissipate energy, thereby further improving the breakdown strength. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] In this embodiment, the linear vinyl silicone oil: the brand is V909619, the viscosity is 90mPa·S (25°C), and it is sourced from Shanghai Maclean Biochemical Technology Co., Ltd.; the branched vinyl silicone oil: the brand is V909621, the viscosity is 90mPa·S (25°C), and it is sourced from Shanghai Maclean Biochemical Technology Co., Ltd.; the monovinyl-terminated methyl silicone oil: the viscosity is 2000mPa·s (25°C), the vinyl mass fraction is 0.16%, and it is sourced from Guangzhou Jucheng Zhaoye Organic Silicon Raw Materials Co., Ltd.; the alumina: spherical Al 2 O 3 , with an average particle size of 1-70μm, sourced from Shanghai Xiangtian Nanomaterials Co., Ltd.; Boron nitride: hexagonal boron nitride, with an average particle size of 10-40μm, sourced from Shanghai Naio Nanotechnology Co., Ltd.; Hydrogen-containing silicone oil: active hydrogen mass fraction of 0.12%, sourced from Zhejiang Runhe Silicone New Materials Co., Ltd.
[0045] In the following examples and comparative examples, 1 part is equal to 1 g.
[0046] Embodiment 1: A method for preparing a high thermal conductive silicone gel, comprising the following process:
[0047] Step S1: 100 parts of vinyl silicone oil (composed of linear vinyl silicone oil and branched vinyl silicone oil in a mass ratio of 1:1) and 300 parts of the composite are uniformly mixed to obtain a base rubber;
[0048] Step S2: 100 parts of base rubber, 3 parts of vinyl-terminated phenyl silicone oil, 2 parts of monovinyl-terminated methyl silicone oil, 1 part of inhibitor and 1 part of platinum catalyst are mixed evenly to obtain material A;
[0049] Step S3: 100 parts of base rubber, 2 parts of monovinyl-terminated methyl silicone oil, and 6 parts of hydrogen-containing silicone oil are mixed evenly to obtain material B;
[0050] Step S4: mixing material A and material B in a mass ratio of 1:1, and performing vacuum degassing to obtain a high thermal conductive silicone gel;
[0051] The preparation method of the complex is as follows:
[0052] Step (1): adjusting the pH value of 0.01 mol / L Tris-HCl buffer solution to 8.5, adding dopamine hydrochloride and mixing evenly to obtain a 3 g / L dopamine solution; adding 200 parts of aluminum oxide to 2000 parts of the dopamine solution and stirring for 22 hours, filtering, washing and drying to obtain polydopamine-modified aluminum oxide;
[0053] Step (2): uniformly mix 100 parts of boron nitride and 5 mol / L sodium hydroxide solution, stir at 70°C for 10 hours, heat to 110°C for reaction for 10 hours, cool to room temperature, wash, filter and dry to obtain hydroxylated boron nitride; uniformly mix 100 parts of hydroxylated boron nitride, 10 parts of mercaptopropyltrimethoxysilane, 200 parts of deionized water and 1000 parts of anhydrous ethanol, adjust the system pH to 4, react at 65°C for 5 hours, filter, wash and dry to obtain mercaptolated boron nitride;
[0054] Step (3): 100 parts of mercapto boron nitride, 50 parts of vinyl epoxy silicone and 30 parts of octavinyl POSS were mixed evenly, 10 parts of photoinitiator were added, and after ultraviolet irradiation (irradiation wavelength 360nm, irradiation time 0.5h, irradiation intensity 35mW / cm 2 ), to obtain boron nitride epoxide;
[0055] Step (4): 200 parts of polydopamine-modified alumina, 100 parts of epoxide boron nitride and 1000 parts of anhydrous ethanol were mixed evenly, and reacted at 50° C. for 4 hours to obtain a composite;
[0056] The preparation method of vinyl epoxy silicone is as follows:
[0057] 50 parts of 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, 55 parts of dimethyldimethoxysilane, 250 parts of anhydrous ethanol and 100 parts of deionized water were mixed evenly, the temperature was raised to 70°C, 0.5 parts of dibutyltin dilaurate were added, the reaction was continued for 3 hours, 60 parts of vinyldimethylethoxysilane were added, the end-capping reaction was continued for 2 hours, and the vinyl epoxy silicone was obtained by vacuum rotary evaporation;
[0058] The preparation method of vinyl terminated phenyl silicone oil is as follows:
[0059] 2 parts of diphenyldimethoxysilane, 3 parts of dimethyldimethoxysilane and 0.05 parts of 37wt% hydrochloric acid solution are mixed evenly, reacted at 65°C for 2h, and an intermediate is obtained after washing, separation and dehydration; under nitrogen protection, the intermediate, 6 parts of divinyltetramethyldisiloxane and 2 parts of octamethylcyclotetrasiloxane are mixed evenly, 0.01 parts of tetramethylammonium hydroxide are added, reacted at 75°C for 3h, and vinyl-terminated phenyl silicone oil is obtained after reduced pressure distillation.
[0060] Embodiment 2: A method for preparing a high thermal conductive silicone gel, comprising the following process:
[0061] Step S1: 105 parts of vinyl silicone oil (composed of linear vinyl silicone oil and branched vinyl silicone oil in a mass ratio of 1:1) and 600 parts of the composite are uniformly mixed to obtain a base rubber;
[0062] Step S2: 105 parts of base rubber, 4 parts of vinyl-terminated phenyl silicone oil, 3 parts of monovinyl-terminated methyl silicone oil, 2 parts of inhibitor and 2 parts of platinum catalyst are mixed uniformly to obtain material A;
[0063] Step S3: 105 parts of base rubber, 3 parts of monovinyl-terminated methyl silicone oil, and 10 parts of hydrogen-containing silicone oil are mixed evenly to obtain material B;
[0064] Step S4: mixing material A and material B in a mass ratio of 1:1, and performing vacuum degassing to obtain a high thermal conductive silicone gel;
[0065] The preparation method of the complex is as follows:
[0066] Step (1): adjusting the pH value of 0.01 mol / L Tris-HCl buffer solution to 8.5, adding dopamine hydrochloride and mixing evenly to obtain a 4 g / L dopamine solution; adding 320 parts of aluminum oxide to 2100 parts of the dopamine solution and stirring for 23 hours, filtering, washing and drying to obtain polydopamine-modified aluminum oxide;
[0067] Step (2): 280 parts of boron nitride and 1200 parts of 8 mol / L sodium hydroxide solution are mixed uniformly, stirred at 75°C for 11 hours, heated to 115°C for reaction for 11 hours, cooled to room temperature, washed, filtered, and dried to obtain hydroxylated boron nitride; 280 parts of hydroxylated boron nitride, 56 parts of mercaptopropyltrimethoxysilane, 840 parts of deionized water and 3500 parts of anhydrous ethanol are mixed uniformly, the system pH is adjusted to 5, reacted at 70°C for 6 hours, filtered, washed, and dried to obtain mercaptolated boron nitride;
[0068] Step (3): 280 parts of mercapto boron nitride, 224 parts of vinyl epoxy silicone and 112 parts of octavinyl POSS were mixed evenly, 56 parts of photoinitiator were added, and after ultraviolet irradiation (irradiation wavelength 380nm, irradiation time 1h, irradiation intensity 25mW / cm 2 ), to obtain boron nitride epoxide;
[0069] Step (4): 320 parts of polydopamine-modified alumina, 280 parts of epoxide boron nitride and 2560 parts of anhydrous ethanol were mixed evenly, and reacted at 55° C. for 5 hours to obtain a composite;
[0070] The preparation method of vinyl epoxy silicone is as follows:
[0071] 250 parts of 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, 280 parts of dimethyldimethoxysilane, 2000 parts of anhydrous ethanol and 750 parts of deionized water were mixed evenly, the temperature was raised to 75°C, 5 parts of dibutyltin dilaurate were added, the reaction was continued for 4 hours, and 325 parts of vinyldimethylethoxysilane were added, the end-capping reaction was continued for 3 hours, and the vinyl epoxy silicone was obtained by vacuum rotary evaporation;
[0072] The preparation method of vinyl terminated phenyl silicone oil is as follows:
[0073] 3 parts of diphenyldimethoxysilane, 4 parts of dimethyldimethoxysilane and 0.08 parts of 37wt% hydrochloric acid solution are mixed evenly, reacted at 70°C for 3h, and an intermediate is obtained after washing, separation and dehydration; under nitrogen protection, the intermediate, 7 parts of divinyltetramethyldisiloxane and 3 parts of octamethylcyclotetrasiloxane are mixed evenly, 0.03 parts of tetramethylammonium hydroxide are added, reacted at 80°C for 5h, and vinyl-terminated phenyl silicone oil is obtained after reduced pressure distillation.
[0074] Embodiment 3: A method for preparing a high thermal conductive silicone gel, comprising the following process:
[0075] Step S1: 110 parts of vinyl silicone oil (composed of linear vinyl silicone oil and branched vinyl silicone oil in a mass ratio of 1:1) and 900 parts of the composite are mixed evenly to obtain a base rubber;
[0076] Step S2: 110 parts of base rubber, 5 parts of vinyl-terminated phenyl silicone oil, 4 parts of monovinyl-terminated methyl silicone oil, 3 parts of inhibitor and 3 parts of platinum catalyst are mixed uniformly to obtain material A;
[0077] Step S3: 110 parts of base rubber, 4 parts of monovinyl-terminated methyl silicone oil, and 12 parts of hydrogen-containing silicone oil are mixed evenly to obtain material B;
[0078] Step S4: mixing material A and material B in a mass ratio of 1:1, and performing vacuum degassing to obtain a high thermal conductive silicone gel;
[0079] The preparation method of the complex is as follows:
[0080] Step (1): adjusting the pH value of 0.01 mol / L Tris-HCl buffer solution to 8.5, adding dopamine hydrochloride and mixing evenly to obtain a 5 g / L dopamine solution; adding 450 parts of aluminum oxide to 2250 parts of the dopamine solution and stirring for 24 hours, filtering, washing and drying to obtain polydopamine modified aluminum oxide;
[0081] Step (2): 450 parts of boron nitride and 2250 parts of sodium hydroxide solution are mixed evenly, stirred at 80°C for 12h, heated to 120°C for reaction for 12h, cooled to room temperature, washed, filtered, and dried to obtain hydroxylated boron nitride; 450 parts of hydroxylated boron nitride, 135 parts of mercaptopropyltrimethoxysilane, 1800 parts of deionized water and 6750 parts of anhydrous ethanol are mixed evenly, the pH of the system is adjusted to 6, reacted at 75°C for 6h, filtered, washed, and dried to obtain mercaptolated boron nitride;
[0082] Step (3): 450 parts of mercapto boron nitride, 360 parts of vinyl epoxy silicone and 225 parts of octavinyl POSS were mixed evenly, 135 parts of photoinitiator were added, and after ultraviolet irradiation (irradiation wavelength 400nm, irradiation time 2.0h, irradiation intensity 20mW / cm 2 ), to obtain boron nitride epoxide;
[0083] Step (4): 450 parts of polydopamine-modified alumina, 450 parts of epoxide boron nitride and 4500 parts of anhydrous ethanol were mixed evenly, and reacted at 60° C. for 6 hours to obtain a composite;
[0084] The preparation method of vinyl epoxy silicone is as follows:
[0085] 360 parts of 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, 432 parts of dimethyldimethoxysilane, 3600 parts of anhydrous ethanol and 1440 parts of deionized water were mixed evenly, the temperature was raised to 80°C, 10.8 parts of dibutyltin dilaurate were added, the reaction was continued for 5 hours, and 504 parts of vinyldimethylethoxysilane were added, the end-capping reaction was continued for 4 hours, and the vinyl epoxy silicone was obtained by vacuum rotary evaporation;
[0086] The preparation method of vinyl terminated phenyl silicone oil is as follows:
[0087] 4 parts of diphenyldimethoxysilane, 5 parts of dimethyldimethoxysilane and 0.10 parts of 37wt% hydrochloric acid solution are mixed evenly, reacted at 75°C for 4 hours, and an intermediate is obtained after washing, separation and dehydration; under nitrogen protection, the intermediate, 8 parts of divinyltetramethyldisiloxane and 4 parts of octamethylcyclotetrasiloxane are mixed evenly, 0.03 parts of tetramethylammonium hydroxide are added, reacted at 80°C for 5 hours, and vinyl-terminated phenyl silicone oil is obtained after reduced pressure distillation.
[0088] Comparative Example 1: A method for preparing a high thermal conductive silicone gel, comprising the following processes:
[0089] Compared with Example 2, in Comparative Example 1, the composite in step S1 is replaced with polydopamine-modified alumina, and the other steps are the same as those in Example 2.
[0090] Comparative Example 2: A method for preparing a high thermal conductive silicone gel, comprising the following processes:
[0091] Compared with Example 2, in step S2 of Comparative Example 2, no vinyl-terminated phenyl silicone oil is added, and the other steps are the same as those of Example 2.
[0092] Comparative Example 3: A method for preparing a high thermal conductive silicone gel, comprising the following processes:
[0093] Compared with Example 2, in Comparative Example 3, the vinyl silicone oil in step S1 is replaced with monovinyl-terminated methyl silicone oil, and the other steps are the same as those in Example 2.
[0094] Comparative Example 4: A method for preparing a high thermal conductive silicone gel, comprising the following processes:
[0095] Compared with Example 2, in step (4) of Comparative Example 4, the mass ratio of polydopamine-modified alumina to epoxide boron nitride is 1:0.2; the other steps are the same as those in Example 2.
[0096] Experiment: The high thermal conductivity silicone gel obtained in Examples 1-3 and Comparative Examples 1-4 was injected into a mold, and after curing at room temperature for 24 hours, a test piece was obtained. The thermal conductivity was tested according to ASTM D5470, and the thickness of the test piece was 2 mm. The Shore 00 hardness test was performed according to ASTM D2240, and the thickness of the test piece was 6 mm. A breakdown strength tester HJC-50kV was used to perform a breakdown test on a test piece with a thickness of 1 mm, and the voltage was increased at a rate of 1 kV / s until the test piece was broken down, and the data was recorded.
[0097] Test Results
[0098]
[0099] According to the data in the above table, we can clearly draw the following conclusions:
[0100] 1. Compared with Examples 1-3, the thermal conductivity and hardness of the product obtained in Comparative Example 1 decreased, indicating that compared with polydopamine-modified alumina, the composite prepared by the present invention has better thermal conductivity and hardness.
[0101] 2. Compared with Examples 1-3, the breakdown strength of the product obtained in Comparative Example 2 is reduced, which indicates that the vinyl-terminated phenyl silicone oil prepared in the present invention can improve the breakdown strength of the silicone gel.
[0102] 3. Compared with Examples 1-3, the thermal conductivity of the products obtained in Comparative Examples 3 and 4 is reduced. It can be seen that increasing the viscosity of the vinyl silicone oil will lead to uneven dispersion of the composite, thereby causing the thermal conductivity of the product to decrease; reducing the amount of epoxide boron nitride added will reduce the thermal conductivity of the silicone gel.
[0103] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0104] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high thermal conductive silicone gel, characterized in that: The steps include: Step S1: uniformly mixing the vinyl silicone oil and the composite to obtain a base rubber; the composite is compounded by polydopamine-modified alumina and epoxide boron nitride; Step S2: uniformly mixing the base rubber, vinyl-terminated phenyl silicone oil, monovinyl-terminated methyl silicone oil, inhibitor and platinum catalyst to obtain material A; Step S3: uniformly mixing the base rubber, monovinyl-terminated methyl silicone oil and hydrogen-containing silicone oil to obtain material B; Step S4: Mix material A and material B evenly, and perform vacuum degassing to obtain a high thermal conductive silicone gel.
2. The method for preparing a high thermal conductive silicone gel according to claim 1, characterized in that: In the step S1, the base glue comprises the following components by weight: 100-110 parts of vinyl silicone oil and 300-900 parts of the composite.
3. The method for preparing a high thermal conductive silicone gel according to claim 2, characterized in that: The vinyl silicone oil is composed of straight-chain vinyl silicone oil and branched-chain vinyl silicone oil in a mass ratio of 1:
1.
4. The method for preparing a high thermal conductivity silicone gel according to claim 2, characterized in that: The preparation method of the composite is as follows: Step (1): adjusting the pH of the Tris-HCl buffer solution to 8.5, adding dopamine hydrochloride and mixing evenly to obtain a dopamine solution; adding alumina to the dopamine solution and stirring for 22-24 hours, filtering, washing, and drying to obtain polydopamine-modified alumina; Step (2): evenly mix the boron nitride and the sodium hydroxide solution, stir at 70-80° C. for 10-12 hours, heat to 110-120° C. for reaction for 10-12 hours, cool to room temperature, wash, filter, and dry to obtain hydroxylated boron nitride; evenly mix the hydroxylated boron nitride, mercaptopropyltrimethoxysilane, deionized water, and anhydrous ethanol, adjust the system pH to 4-6, react at 65-75° C. for 5-7 hours, filter, wash, and dry to obtain thiolated boron nitride; Step (3): uniformly mixing the mercapto boron nitride, vinyl epoxy silicone and octavinyl POSS, adding a photoinitiator, and irradiating with ultraviolet light to obtain epoxide boron nitride; Step (4): uniformly mix polydopamine-modified alumina, epoxide boron nitride and anhydrous ethanol, and react at 50-60° C. for 4-6 hours to obtain a composite.
5. The method for preparing a high thermal conductive silicone gel according to claim 4, characterized in that: In the step (1), the concentration of the Tris-HCl buffer is 0.01 mol / L, the concentration of the dopamine solution is 3-5 g / L, and the mass of the aluminum oxide is 10-20% of the mass of the dopamine solution.
6. The method for preparing a high thermal conductive silicone gel according to claim 4, characterized in that: In the step (3), the preparation method of vinyl epoxy silicone is as follows: Mix 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, dimethyldimethoxysilane, anhydrous ethanol and deionized water evenly, heat to 70-80°C, add dibutyltin dilaurate, react for 3-5h, then add vinyldimethylethoxysilane, capping reaction for 2-4h, and obtain vinyl epoxy silicone by vacuum rotary evaporation.
7. The method for preparing a high thermal conductive silicone gel according to claim 1, characterized in that: In step S2, material A includes the following components by weight: 100-110 parts of base rubber, 3-5 parts of vinyl-terminated phenyl silicone oil, 2-4 parts of monovinyl-terminated methyl silicone oil, 1-3 parts of inhibitor, and 1-3 parts of platinum catalyst.
8. The method for preparing a high thermal conductive silicone gel according to claim 7, characterized in that: The preparation method of the vinyl-terminated phenyl silicone oil is as follows: Diphenyldimethoxysilane, dimethyldimethoxysilane and hydrochloric acid solution are mixed evenly, reacted at 65-75°C for 2-4h, and washed, separated and dehydrated to obtain an intermediate; under nitrogen protection, the intermediate, divinyltetramethyldisiloxane and octamethylcyclotetrasiloxane are mixed evenly, tetramethylammonium hydroxide is added, reacted at 75-80°C for 3-5h, and distilled under reduced pressure to obtain vinyl-terminated phenyl silicone oil.
9. The method for preparing a high thermal conductive silicone gel according to claim 1, characterized in that: In step S3, material B includes the following components by weight: 100-110 parts of base rubber, 2-4 parts of monovinyl-terminated methyl silicone oil, and 6-12 parts of hydrogen-containing silicone oil.
10. A high thermal conductive silicone gel prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Thermally-stable two-component heat-conducting gel and preparation method thereof
CN115216154A
Single-component heat-conducting silica gel as well as preparation method and application thereof
CN116178964A
High-strength low-dielectric-constant printed circuit board and preparation process thereof
CN117042327A
Two-component heat-conducting pouring sealant for OBC charging module and preparation method of two-component heat-conducting pouring sealant
CN117384584A
Preparation method for improving thermal conductivity of epoxy resin based on core-shell structure
CN117624833A
Cited By
Bonding type anti-yellowing organic silicon gel, preparation method thereof, tackifier used in bonding type anti-yellowing organic silicon gel and preparation method of tackifier
CN116751366A
Aminophenyl co-modified silicone oil as well as preparation method and application thereof
CN120137174A
High-temperature-resistant heat-conducting oil and preparation method thereof
CN121064803A