Preparation and application of green marine antifouling coating based on quaternary ammonium salt chitosan
Through layer-by-layer self-assembly technology of quaternary ammonium chitosan and polyanionic polysaccharides, a marine antifouling coating with self-regulating degradation rate is constructed, which solves the antifouling effect of marine antifouling coatings in the existing technology under low speed or static environments. The poor problem has achieved efficient anti-fouling performance and environmentally friendly applications in different marine environments.
Patent Information
- Application Number
- CN202411150818.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing marine antifouling coatings are difficult to maintain an ideal antifouling state on low-speed or static marine structures, and lack effective self-regulating degradation rates, resulting in a decrease in antifouling effect.
Quaternary ammonium chitosan and polyanionic polysaccharides are constructed through layer-by-layer self-assembly method to form a green marine antifouling coating with anti-protein adhesion, anti-microbial adhesion and dirt release capabilities, so as to achieve the Self-regulated degradation rate in different marine environments.
The coating exhibits excellent anti-fouling performance in both static and dynamic environments, significantly reducing the adhesion of proteins and microorganisms, and has self-regulated degradation characteristics. It is suitable for widespread use in marine ships and underwater equipment, reducing production costs and avoiding Environmental pollution.
Smart Images

Figure CN118909489A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of marine antifouling, and relates to the preparation and application of a green marine antifouling coating based on quaternary ammonium salt chitosan. Background Art
[0002] How to prevent marine organisms from attaching to and corroding the hull has always been a key issue in the field of navigation. Marine biofouling, also known as marine fouling, refers to the unnatural attachment and growth of various marine organisms, including algae, bacteria, protozoa, sponges, coelenterates, mollusks, echinoderms, etc., on the surface of underwater structures such as hulls, submarine pipelines, and offshore platforms. This type of fouling has many harmful effects on human activities and the marine ecological environment, mainly including: (1) Increased resistance and energy consumption: On ships, the attachment of marine organisms will significantly increase the roughness of the underwater surface, thereby increasing navigation resistance, resulting in increased fuel consumption and rising operating costs. (2) Damage to marine facilities: Fouling organisms can clog equipment such as pipes and filters, affecting normal operation, accelerating the corrosion of metal structures, and shortening the service life of marine facilities, such as offshore oil and gas platforms, desalination plants, and fishery facilities. (3) Interference with marine instruments and machinery: Attached organisms may cover key components such as sensors and valves, causing the function of marine observation and production equipment to fail, affecting the accuracy of data or the safe operation of equipment. (4) Harm to aquaculture: In cage culture and raft culture, fouling organisms will occupy the breeding space, compete for oxygen and nutrients, and even directly harm the cultured organisms, reducing the yield and quality. (5) Disruption of ecological balance: Alien or overgrown fouling species may become invasive species, threaten native species, change the structure and function of the ecosystem, and affect biodiversity. (6) Economic losses: Marine fouling needs to be cleaned up regularly, which involves high human and material costs. At the same time, the reduction in production efficiency caused by fouling will also bring economic losses. (7) Health risks: Some fouling organisms may be carriers of pathogens, which may be transmitted to humans through the food chain, posing a public health risk.
[0003] Applying marine antifouling paint on the hull is currently the main solution to biofouling. With the improvement of global awareness of environmental protection, the technical trend of marine antifouling paint is evolving towards a greener and more environmentally friendly direction. This shift requires the paint to reduce or eliminate environmentally harmful components, such as organotin compounds, high concentrations of cuprous oxide, heavy metal fungicides, or even completely abandon traditional fungicides. At present, Wuxi self-polishing antifouling paint dominates the market due to its significant environmental advantages and excellent antifouling performance. This type of paint not only avoids the high toxicity problem of organotin paint, but also inherits the excellent properties of self-polishing paint, that is, through the ion exchange mechanism in seawater, the polymer is dissolved, and then the antifouling agent is released to achieve a continuous antifouling effect. The mainstream Wuxi self-polishing paint system includes polymer coatings based on copper acrylate, zinc acrylate and acrylate silane esters. The anti-hydrolysis properties of these coatings ensure that hydrolysis will only occur when the surface resin is in direct contact with seawater, so that the surface is converted from hydrophobic to hydrophilic, and then slowly and continuously dissolved, ensuring the continuous release of antifouling agents and maintaining antifouling performance. Nevertheless, this type of coating has an obvious limitation in application - their performance depends to a certain extent on the scouring effect of water flow, especially when the ship is stationary, due to the lack of sufficient water flow stimulation, the renewal rate of the coating is reduced, and the antifouling effect is greatly reduced. This defect limits their application in slow-moving ships, submarines and fixed offshore facilities such as oil drilling platforms, because the coating cannot be fully renewed in these cases and it is difficult to maintain an ideal antifouling state. In order to overcome this limitation, the present invention aims to provide a new type of antifouling coating with the characteristic of self-regulating degradation rate according to the environment, so as to meet the needs of different marine operating environments, especially those slow-speed or static marine structures, to ensure that continuous and effective antifouling protection can be provided under any circumstances.
[0004] Natural polysaccharides are the most abundant natural polymers on earth and have good biocompatibility and degradability. At the same time, polysaccharides have a high degree of hydrophilicity and hydration due to the large number of carboxyl, hydroxyl and amino groups, which makes many polysaccharides have the ability to resist protein adsorption, bacterial adhesion and cell adhesion. Chitosan is a linear polysaccharide composed of randomly distributed β-(1,4)-linked D-glucosamine (deacetylated units) and N-acetyl-D-glucosamine (acetylated units). Chitosan is the product of partial deacetylation of chitin, a naturally occurring polysaccharide that exists in large quantities in the exoskeletons of marine arthropods such as crustaceans, the shells of insects, the cell membranes of fungi and algae, the shells of mollusks, and the bones of higher plants. Quaternized chitosan is a product of quaternized chitosan, in which the hydroxyl groups of chitosan are replaced by quaternary ammonium groups (positive ions) to form quaternized chitosan with a positive charge. The following characteristics of quaternary ammonium chitosan give it advantages in the field of antifouling: (1) Positive charge properties: The quaternary ammonium group gives quaternary ammonium chitosan a positive charge, which makes it have good solubility and adsorption. The positive charge enables it to interact with negatively charged substances, such as negative ions on the surface of bacteria, negatively charged drugs, etc. (2) Due to the cationic nature of its quaternary ammonium group, quaternary ammonium chitosan can interact with negative ions on the surface of bacteria, resulting in the destruction of bacterial membranes and leakage of intracellular substances, thereby achieving a bactericidal effect. This bactericidal mechanism is widely used in the fields of medicine, food and disinfection. (3) Biocompatibility: Similar to chitosan, quaternary ammonium chitosan also has good biocompatibility and biodegradability. This makes it used as a degradable medical material and tissue engineering scaffold in the fields of medicine and tissue engineering. (4) Corrosion inhibition: Some studies have shown that surface quaternary ammonium chitosan can also inhibit the corrosion process of materials such as carbon steel through its adsorption as a corrosion inhibitor that can simultaneously delay both cathodic and anodic processes.
[0005] Polyelectrolyte multilayers (PEMs) are multilayer films formed by charged polymers (polyelectrolytes) deposited layer by layer on a solid surface through electrostatic interactions. Its thickness is generally between a few nanometers and hundreds of nanometers, and it can be used to prepare various functional materials and devices. PEMs have good controllability and adaptability, and different structures, morphologies and properties can be designed according to needs. They are widely used in biomedicine, electronic devices, sensors and other fields. The preparation of polyelectrolyte multilayers usually adopts the layer-by-layer self-assembly method (layer-by-layer deposition, LBL) of ion alternating deposition. The thin films or coating materials prepared by the LBL method have the advantages of strong controllability, good applicability to unconventional surfaces and diverse functionality, and the high salt stability of the LBL membrane can be enhanced by selecting polyelectrolyte pairs with high binding strength.
[0006] Chinese patent CN114904402B discloses a layer-by-layer self-assembled sustained-release antibacterial polymer separation membrane and its preparation method and application. The preparation method of the present invention comprises: immersing the polymer separation membrane in a mixed solution of polyphenolic compounds and polyethyleneimine to functionalize its surface; then utilizing the physical adsorption and electrostatic effect between negatively charged polysaccharides and positively charged antimicrobial peptides, loading polysaccharides and antimicrobial peptides on the surface of the base membrane by layer-by-layer self-assembly to obtain a polymer separation membrane with antibacterial and anti-biological pollution properties. The modified polymer separation membrane has significantly improved antibacterial and anti-pollution capabilities, and has a significant inhibitory effect on the reproduction of bacteria and microorganisms. The present invention adopts layer-by-layer self-assembly technology for antibacterial modification, has a mild reaction, is simple to operate, and the prepared polymer separation membrane modified layer is adjustable, has good antibacterial and anti-pollution properties, and has good application prospects in the field of water treatment. However, this patent also has the following disadvantages: (1) High cost: the production of antimicrobial peptides involves relatively complex biosynthesis or chemical synthesis; Poor durability: (2) Antimicrobial peptides may be enzymatically hydrolyzed by microorganisms in certain circumstances, making it difficult to maintain the antimicrobial effect for a long time. Summary of the invention
[0007] The purpose of the present invention is to provide a preparation method and application of a green marine antifouling coating based on quaternary ammonium salt chitosan, which has the ability of resisting protein adhesion, antimicrobial adhesion and dirt release in a marine environment. The present invention adopts quaternary ammonium salt chitosan and polyanion polysaccharide, and constructs a polysaccharide polyelectrolyte multilayer film by a layer-by-layer self-assembly method, which is used as a marine antifouling coating material. The polysaccharide composite antifouling coating material shows good anti-adhesion performance in protein solution and Chlorella suspension, has a controllable degradation rate and self-polishing performance in seawater, and can be widely used in the antifouling of underwater equipment such as marine ships, warships and docks.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] The first aspect of the present invention provides a method for preparing a green marine antifouling coating based on quaternary ammonium chitosan, comprising: immersing a substrate in a quaternary ammonium chitosan solution and an anionic polysaccharide solution in sequence, and repeating the process to self-assemble layer by layer, and drying to obtain the green marine antifouling coating.
[0010] Furthermore, the preparation method of the quaternary ammonium salt chitosan comprises: heating chitosan and 2,3-epoxypropyltrimethylammonium chloride to react to obtain quaternary ammonium salt chitosan;
[0011] The mass ratio of the chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:(1-5).
[0012] Furthermore, the weight average molecular weight M of the chitosan WThe range is 5000-50000, and the degree of deacetylation is ≥95%.
[0013] Furthermore, in the heating reaction, the reaction temperature is 60-90° C. and the reaction time is 2-10 h.
[0014] As a preferred technical solution, in the heating reaction, the reaction solvent is isopropanol. The preferred stirring rate is 100-500 rpm.
[0015] As a preferred technical solution, after the heating reaction, the obtained product is separated, dialyzed and freeze-dried to remove unreacted quaternary ammonium salt reagent (2,3-epoxypropyltrimethylammonium chloride), isopropanol and the like.
[0016] As a preferred technical solution, in the separation dialysis, the minimum molecular weight cutoff of the dialysis bag used is 500-5000, and the dialysis time is 3-5 days.
[0017] Furthermore, the anionic polysaccharide is selected from at least one of carrageenan, sodium alginate, xanthan gum, gellan gum, welan gum, hyaluronic acid, pectin, sodium carboxymethyl cellulose, carboxymethyl starch, carboxymethyl curdlan, carboxymethyl konjac gum, carboxymethyl guar gum or carboxymethyl xyloglucan.
[0018] Furthermore, the mass concentration of the quaternary ammonium salt chitosan solution is 0.5-2%, and the pH is 4.5-6.5;
[0019] The mass concentration of the anionic polysaccharide solution is 0.5-2%, and the pH value is 4.5-6.5.
[0020] As a preferred technical solution, the pH of the quaternary ammonium salt chitosan solution or the anionic polysaccharide solution is adjusted by using HCl solution and NaOH solution with a molar concentration of 1 mol / L.
[0021] Furthermore, the substrate is one of a cement substrate, a metal substrate or a glass fiber substrate.
[0022] Furthermore, in the quaternary ammonium chitosan solution or anionic polysaccharide solution, the substrate is immersed at room temperature for 5-15 minutes, the cycle is repeated 50-100 times, the first immersion solution is anionic polysaccharide solution, and the last immersion solution is quaternary ammonium chitosan solution.
[0023] Furthermore, after each immersion, the substrate is washed with a NaCl / HCl aqueous solution having a pH of 4.5-6.5, wherein the NaCl concentration is 0.1-0.5 mol / L.
[0024] Furthermore, in the drying, the drying temperature is 40-70° C. and the drying time is 12-24 hours.
[0025] A second aspect of the present invention provides an application of a green marine antifouling coating, including using the green marine antifouling coating for antifouling treatment of underwater equipment.
[0026] Compared with the prior art, the present invention has the following characteristics:
[0027] 1) Using natural polysaccharides as raw materials, a green marine antifouling coating was successfully synthesized through a simple layer-by-layer self-assembly method. The prepared coating exhibited excellent static and dynamic antifouling capabilities.
[0028] 2) Compared with the current polymer resin antifouling coating based on small molecule antifouling agents and low surface energy antifouling coating based on organosilicon and organofluorine, this coating achieves a better antifouling effect by introducing a multi-element antifouling mechanism. First, the good hydrophilicity and hydration of polysaccharides are used to achieve the ability to resist protein adhesion. Secondly, the antibacterial ability of the coating is enhanced by introducing quaternary ammonium salt groups. Finally, the coating has different degradation rates in different marine environments, and the self-regulating characteristics of the coating are achieved, which is a slow degradation when there are few attachments and a high degradation when there are many attachments.
[0029] 3) The green marine antifouling coating prepared by the present invention has demonstrated its excellent antifouling performance through a series of rigorous performance evaluations. In the anti-protein adhesion test, the coating material demonstrated a reduction of more than 90% in adhesion to common proteins, a result that highlights the coating's high efficiency in resisting biomolecule adsorption. In addition, in the antibacterial performance test, the coating also performed well, proving that it can significantly reduce the attachment rate of common microorganisms by up to 95%, which directly reflects the coating material's strong ability to inhibit microbial growth and reproduction.
[0030] 4) The preparation process does not use or produce pollutants such as waste acid and waste alkali that are harmful to the environment, and the process is simple, green and environmentally friendly, and suitable for industrial application;
[0031] 5) The present invention adopts quaternary ammonium salt chitosan as antibacterial material. Compared with the slow-release antibacterial polymer based on antimicrobial peptides in the prior art, the advantage is that quaternary ammonium chitosan is widely available, usually prepared by chemical modification of natural chitosan, with low production cost, and chitosan is widely present in the marine environment, and its degradation products do not cause harm to the marine environment. The production of antimicrobial peptides involves more complex biosynthesis or chemical synthesis, and the cost is relatively high. Secondly, quaternary ammonium chitosan can effectively act on negatively charged bacterial cell membranes due to its positively charged quaternary ammonium group, resulting in the destruction of bacterial cell membranes, thereby achieving a long-lasting antibacterial effect. Antimicrobial peptides may be enzymolyzed by microorganisms in some cases, and the antibacterial effect may not be as lasting as quaternary ammonium chitosan. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1It is a comparative infrared spectrum of chitosan and the quaternary ammonium salt chitosan described in Example 1.
[0033] Figure 2 This is a scanning electron microscope image of the marine antifouling coating prepared in Example 1.
[0034] Figure 3 This is a graph showing the results of the protein antifouling performance evaluation experiment of the marine antifouling coating of Example 2 of the present invention for anti-protein adhesion testing.
[0035] Figure 4 This is a graph showing the anti-biological attachment test results of the marine antifouling coating of Example 3 in the microbial antifouling performance test experiment of the present invention.
[0036] Figure 5 This is a graph showing the degradation results of the marine antifouling coating of Example 4 in the coating degradation performance measurement experiment of the present invention in different simulated marine environments. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0038] Embodiment 1:
[0039] This embodiment provides a method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan with a multi-element antifouling mechanism, comprising the following steps:
[0040] (1) The ingredients were prepared according to the mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride being equal to 1:2. The 2,3-epoxypropyltrimethylammonium chloride solution was slowly added dropwise to the isopropanol suspension of chitosan in a constant temperature water bath at 80° C. The reaction lasted for 6 hours with a stirring rate of 200 rpm. The weight average molecular weight of the chitosan used was about 10,000.
[0041] (2) The isopropanol in the upper layer was removed by decantation, and the product was placed in a dialysis bag with a molecular weight cutoff of 500. After dialysis for 3 days, the product was freeze-dried.
[0042] (3) The synthesized quaternary ammonium salt chitosan sample and carrageenan sample were prepared into polysaccharide aqueous solution with a concentration of 1wt%, and the pH of the quaternary ammonium salt chitosan solution and carrageenan solution was adjusted to 5.5 using a sodium hydroxide solution with a concentration of 1% by mass. First, the adhesive glass sheet (25mm×75mm, thickness 1.0mm, purchased from Shanghai Titan Technology Co., Ltd.) with surface positive charge treatment was immersed in the carrageenan solution for 5min, and then the surface was washed with a 0.15M NaCl aqueous solution adjusted to pH 5.5 with a 1mol / L HCl solution, and then the adhesive glass sheet was immersed in the quaternary ammonium salt chitosan solution for 5min, and the washing and deposition steps were repeated 50 times (carrageenan solution immersion→NaCl solution washing→quaternary ammonium salt chitosan solution immersion→carrageenan solution immersion→…→quaternary ammonium salt chitosan solution immersion), and finally the glass was placed in a constant temperature drying oven at 80℃ for 24h to obtain the coating material on the glass surface.
[0043] The quaternary ammonium salt chitosan prepared in Example 1 and the prepared coating material were structurally characterized by the following test method:
[0044] (1) Material structure analysis: Fourier transform infrared spectroscopy (FTIR) technology was used to compare and analyze the chemical structure differences between the original chitosan and the chitosan modified by quaternary ammonium salt to confirm the successful introduction of the quaternary ammonium salt group.
[0045] (2) Observation of coating microstructure: Scanning electron microscopy (SEM) was used to perform high-resolution imaging of the prepared coating surface to intuitively display the microstructure and morphological characteristics of the coating.
[0046] The structural characterization results are as follows:
[0047] Figure 1 The infrared spectra of chitosan (CTS) and quaternary ammonium salt chitosan (N-CTS) prepared in Example 1 are compared. Figure 1 It can be seen that chitosan has a weak absorption area of 2878 cm -1 The weak absorption peak at 1652cm is the stretching peak of CH. -1 and 1550cm -1 The C=O stretching vibration of amide I and the δN-H bending vibration of amide II are 1420 cm -1 The deformation absorption peak of -CH3 is 1071cm -1 and 1028cm -1 The secondary alcohol hydroxyl stretching vibration and the primary alcohol hydroxyl stretching vibration are 897cm -1 The absorption peak at 1480cm is the absorption peak of the sugar ring structure group. In contrast, some significant changes appeared in the infrared spectrum of the quaternary ammonium salt chitosan sample. First, at 1480cm-1 A new strong absorption peak appeared at 1642 cm, which can be attributed to the CH bending vibration peak on the trimethylamine group, indicating that quaternary ammonium groups were introduced into the chitosan sample. -1 The absorption at 897 cm-1 increased, indicating that some of the primary amines have been converted into secondary amines. -1 The peak at 917 cm -1 A new absorption peak appeared at , indicating that the introduction of quaternary ammonium salt groups led to the change of the molecular structure of chitosan.
[0048] Figure 2 This is the SEM result of the cross section of the marine antifouling coating prepared in Example 1. It shows that the obtained material has obtained the typical multi-layer microstructure expected by the scheme.
[0049] Embodiment 2:
[0050] This embodiment provides a method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan with a multi-element antifouling mechanism, comprising the following steps:
[0051] (1) The ingredients were prepared according to the mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride being equal to 1:3. The 2,3-epoxypropyltrimethylammonium chloride solution was slowly added dropwise to the isopropanol suspension of chitosan in a constant temperature water bath at 80° C. The reaction lasted for 8 hours with a stirring rate of 500 rpm. The weight average molecular weight of the chitosan used was 20,000.
[0052] (2) The isopropanol in the upper layer was removed by decantation, and the product was placed in a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 3 days, the product was freeze-dried.
[0053] (3) The synthesized quaternary ammonium salt chitosan sample and the hyaluronic acid sample were prepared into a polysaccharide aqueous solution with a concentration of 0.5wt%, and the pH of the quaternary ammonium salt chitosan solution and the hyaluronic acid solution was adjusted to 5.5 using a sodium hydroxide solution with a concentration of 1% by mass. First, an epoxy glass fiber sheet (FR-4, purchased from Shanghai Nanjue New Material Technology Co., Ltd.) was immersed in the hyaluronic acid solution for 10 minutes, and after being taken out, the surface was washed with a 0.15M NaCl aqueous solution adjusted to pH 5.5 with a 1mol / L HCl solution, and then the epoxy glass fiber sheet was immersed in the quaternary ammonium salt chitosan solution for 10 minutes, and the washing and deposition steps were repeated 100 times. Finally, the glass was placed in a 60°C constant temperature drying oven for drying for 24 hours to obtain the coating material on the surface of the epoxy glass fiber sheet.
[0054] The protein antifouling performance evaluation experiment was carried out on the marine antifouling coating prepared in Example 2, and the experimental method was as follows:
[0055] Evaluation of protein antifouling performance: The quartz crystal microbalance (QCM-D) technology is used to measure the adhesion behavior of different types of proteins on the coating surface, and the adhesion kinetic curve is drawn to evaluate the anti-protein adhesion performance of the coating.
[0056] The results of the protein antifouling performance evaluation experiment are as follows:
[0057] Figure 3 The results of the protein resistance test of the marine antifouling coating prepared in Example 2 are shown in Figure 2. The adhesion of three common proteins (lysozyme, bovine serum albumin, and fibrinogen) to the epoxy glass fiber sheet without any treatment and the substrate coated with the marine antifouling coating prepared in Example 2 was compared by using a quartz crystal microbalance. The results show that compared with the original substrate, after coating the marine antifouling coating, the adhesion of the three proteins is significantly reduced, among which the adhesion of lysozyme decreases by 95.7%, the adhesion of bovine serum albumin decreases by 96.2%, and the adhesion of fibrinogen decreases by 94.5%, showing excellent protein resistance.
[0058] Embodiment 3:
[0059] This embodiment provides a method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan with a multi-element antifouling mechanism, comprising the following steps:
[0060] (1) The ingredients were prepared according to the mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride being equal to 1:4. The 2,3-epoxypropyltrimethylammonium chloride solution was slowly added dropwise to the isopropanol suspension of chitosan in a constant temperature water bath at 80° C. The reaction lasted for 8 hours with a stirring rate of 300 rpm. The weight average molecular weight of the chitosan used was 20,000.
[0061] (2) The isopropanol in the upper layer was removed by decantation, and the product was placed in a dialysis bag with a molecular weight cutoff of 500. After dialysis for 3 days, the product was freeze-dried.
[0062] (3) The synthesized quaternary ammonium salt chitosan sample and the sodium alginate sample were prepared into a polysaccharide aqueous solution with a concentration of 2wt%, and the pH of the quaternary ammonium salt chitosan solution and the sodium alginate solution was adjusted to 4.5 using a sodium hydroxide solution with a concentration of 1% by mass. First, the carbon steel metal sheet was immersed in the sodium alginate solution for 5 minutes, and after being taken out, the surface was washed with a 0.15M NaCl aqueous solution with a pH adjusted to 4.5 by a 1mol / L HCl solution, and then the carbon steel metal sheet was immersed in the quaternary ammonium salt chitosan solution for 5 minutes, and the washing and deposition steps were repeated 50 times. Finally, the glass was placed in a constant temperature drying oven at 80°C for drying for 24 hours to obtain the coating material on the surface of the carbon steel metal sheet.
[0063] The microbial antifouling performance test experiment was carried out on the marine antifouling coating prepared in Example 3, and the experimental method was as follows:
[0064] Microbial antifouling performance test: The coating samples were placed in a microalgae (Chlorella) culture medium containing 60,000 cells / mL (10 ml of Chlorella species mixed with 50 ml of seawater f / 2 culture medium, both the algae species and the culture medium were purchased from the Seaweed Germplasm Bank of the Chinese Academy of Sciences). After 5 days of static immersion, the microbial attachment on the coating surface was observed and recorded using an optical microscope to evaluate the microbial antifouling effect of the coating.
[0065] The results of the microbial antifouling performance test are as follows:
[0066] Figure 4 The test results of the microbial antifouling performance of the marine antifouling coating prepared in Example 3 are shown. The attachment of Chlorella to ordinary glass and glass coated with the marine antifouling coating prepared in Example 3 after being left in a Chlorella solution for 5 days was compared. The results show that compared with ordinary glass, the glass coated with the marine antifouling coating prepared in Example 3 can effectively reduce the number of Chlorella attached, showing excellent antibacterial properties.
[0067] Embodiment 4:
[0068] This embodiment provides a method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan with a multi-element antifouling mechanism, comprising the following steps:
[0069] (1) The ingredients were prepared according to the mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride being equal to 1:3. The 2,3-epoxypropyltrimethylammonium chloride solution was slowly added dropwise to the isopropanol suspension of chitosan in a constant temperature water bath at 80° C. The reaction lasted for 8 hours with a stirring rate of 500 rpm. The weight average molecular weight of the chitosan used was 20,000.
[0070] (2) The isopropanol in the upper layer was removed by decantation, and the product was placed in a dialysis bag with a molecular weight cutoff of 1000. After dialysis for 3 days, the product was freeze-dried.
[0071] (3) The synthesized quaternary ammonium salt chitosan sample and the xanthan gum sample were prepared into a polysaccharide aqueous solution with a concentration of 1.5wt%, and the pH of the quaternary ammonium salt chitosan solution and the xanthan gum solution was adjusted to 6.5 using a sodium hydroxide solution with a concentration of 1% by mass. First, the adhered glass sheet (25mm×75mm, thickness 1.0mm, purchased from Shanghai Titan Technology Co., Ltd.) with a positive surface charge treatment was immersed in the xanthan gum solution for 10 minutes, and then the surface was washed with a 0.15M NaCl aqueous solution adjusted to pH 6.5 with a 1mol / L HCl solution, and then the adhered glass sheet was immersed in the quaternary ammonium salt chitosan solution for 10 minutes, and the washing and deposition steps were repeated 100 times. Finally, the glass was placed in a constant temperature drying oven at 80°C for 24 hours to obtain a coating material on the glass surface.
[0072] The degradation performance test of the marine antifouling coating prepared in Example 4 was carried out, and the test method was as follows:
[0073] Determination of coating degradation performance: Under simulated marine environmental conditions (such as salinity, pH value, shear rate), the degradation rate and extent of the coating are monitored to evaluate the stability and self-polishing properties of the coating in the actual marine environment.
[0074] The degradation performance test results are as follows:
[0075] Figure 5The degradation results of the marine antifouling coating prepared in Example 4 are compared. The degradation degree of the coating material in 1440 hours under different test conditions, including water flow with different rotation speeds (RS, unit rpm) and seawater with different pH values (simulated seawater ratio is 26.518g / L NaCl, 3.305g / LMgSO4, 2.447g / L MgCl2, 1.141g / LCaCl2, 0.725g / L KCl, 0.202g / L NaHCO3, 0.083g / L NaBr, and the pH is adjusted by using a 1% NaOH solution). Under static simulated seawater conditions, after 1440 hours, the remaining mass (RM, Remain mass) of the coating is 79.9% of the initial mass. When the simulated seawater is stirred with a stirrer at 200rpm, the coating mass drops to 74.6%, indicating that under static and natural seawater flow conditions, the coating degradation rate is slow and the stability is good. When the speed was increased to 500 rpm, the coating degradation rate was 48.0%, indicating that the coating degradation rate was accelerated under stronger seawater shear, which is consistent with the expected degradation effect of self-degradable coatings. Under 500 rpm rotation conditions, reducing the pH of simulated seawater from 8.2 to 6.0 and 4.0 significantly increased the degradation rate of the coating. As the pH decreased, the degradation rate accelerated, and the residual coating mass was 14.7% and 0.1%, respectively. This shows that the effect of the acidic environment on the degradation of the coating is significant. This means that when marine organisms such as barnacles attach, the acidic environment that gradually accumulates during their metabolism promotes the degradation of the coating, thereby promoting the accelerated release of fouling.
[0076] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan, characterized in that: include: The substrate is immersed in a quaternary ammonium salt chitosan solution and an anionic polysaccharide solution in sequence, and the process is repeated layer by layer for self-assembly, and then dried to obtain a green marine antifouling coating.
2. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 1, characterized in that: The preparation method of quaternary ammonium salt chitosan comprises: heating chitosan and 2,3-epoxypropyltrimethylammonium chloride to react to obtain quaternary ammonium salt chitosan; The mass ratio of the chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:(1-5).
3. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 2, characterized in that: The weight average molecular weight M of the chitosan W The range is 5000-50000, and the degree of deacetylation is ≥95%.
4. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 2, characterized in that: In the heating reaction, the reaction temperature is 60-90° C. and the reaction time is 2-10 h.
5. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 1, characterized in that: In the anionic polysaccharide solution, the anionic polysaccharide used is selected from at least one of carrageenan, sodium alginate, xanthan gum, gellan gum, welan gum, hyaluronic acid, pectin, sodium carboxymethyl cellulose, carboxymethyl starch, carboxymethyl curdlan, carboxymethyl konjac gum, carboxymethyl guar gum or carboxymethyl xyloglucan.
6. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 1, characterized in that: The mass concentration of the quaternary ammonium salt chitosan solution is 0.5-2%, and the pH is 4.5-6.5; The mass concentration of the anionic polysaccharide solution is 0.5-2%, and the pH value is 4.5-6.
5.
7. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 1, characterized in that: The substrate is one of a cement substrate, a metal substrate or a glass fiber substrate.
8. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 1, characterized in that: In the quaternary ammonium salt chitosan solution or anionic polysaccharide solution, the substrate is immersed at room temperature for 5-15 minutes, the cycle is repeated 50-100 times, the first immersion solution is anionic polysaccharide solution, and the last immersion solution is quaternary ammonium salt chitosan solution.
9. The method for preparing a green marine antifouling coating based on quaternary ammonium salt chitosan according to claim 1, characterized in that: After each immersion, the substrate was washed with a NaCl / HCl aqueous solution having a pH of 4.5-6.5, wherein the NaCl concentration was 0.1-0.5 mol / L.
10. An application of a green marine antifouling coating prepared by the method according to any one of claims 1 to 9, characterized in that: The green marine antifouling coating is used for antifouling treatment of underwater equipment.
Citation Information
Patent Citations
Self-assembly nano-particles of sulfhydrylation chitosan quaternary ammonium salt and preparation method and application thereof
CN101940551A
Aqueous low-surface-energy antifouling coating material, preparation method and applications thereof
CN110643278A
Non-toxic marine ship antifouling coating material and preparation method thereof
CN111793431A
Multifunctional electrostatic spinning composite nanofiber material as well as preparation method and application thereof
CN115634305A
All-bio-based amphoteric polyelectrolyte antifouling coating as well as preparation method and application thereof
CN117430984A
Cited By
Preparation method and application of novel LBL marine biomass hydrogel composite membrane
CN119701662A
Preparation method and application of a novel LBL marine biomass hydrogel composite membrane
CN119701662B
Organic-inorganic composite pipeline thermal insulation material as well as preparation method and application thereof
CN119931308A
Special phosphorus-free zinc-free seawater scale and corrosion inhibitor and preparation method thereof
CN120887559A
Composite acrylic acid low-surface-energy antifouling coating, preparation method and application
CN121045897A