Cellulose environment-friendly decorative material and preparation method thereof

By using plant powder and wood powder in the coating to form a mesh-like structure, combining the primer layer and the cover layer, the hardness and environmental protection problems of the existing paint are solved, and the softness and environmental protection are improved, and construction is avoided. Dust hazards and improves decorative effects and material durability.

CN118909492APending Publication Date: 2024-11-08QIONGLAI MUZHI ANJU ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411004040.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing coating products are not integrated with the emulsion and water-based components, resulting in hard surfaces, prone to rupture, lack tensile resistance and environmental protection, and contain carcinogenic formaldehyde, which is harmful to the human body and the environment. Dust during construction causes harm to health and the environment. .

Method used

Plant powder and wood powder are used to form a mesh-like structure, combined with primer glue layer and cover layer, through specific coating steps and glue formula, the softness, environmental protection and intergeneration of the paint are improved to form mesh-like paint. Enhance wear resistance, water resistance and fire resistance.

Benefits of technology

It realizes the softness and environmental protection of the paint, avoids cracks and falls off on the surface of the paint, reduces construction dust hazards, improves the decorative effect and material durability, and ensures good adhesion and waterproof performance between the wall and the decorative material. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962480700000101
    Figure BDA0004962480700000101
  • Figure BDA0004962480700000111
    Figure BDA0004962480700000111
  • Figure BDA0004962480700000112
    Figure BDA0004962480700000112
Patent Text Reader

Abstract

The invention discloses a cellulose environment-friendly decorative material and a preparation method thereof, and relates to the field of coatings and preparation methods thereof.The cellulose environment-friendly decorative material comprises a primer adhesive layer, a primer layer, a finishing coat layer and a finishing coat layer which are sequentially connected in a stacked mode, and the primer adhesive layer is used for being connected with a building wall surface; wherein both the primer layer and the finish paint layer contain plant powder and wood powder. According to the invention, the primer layer and the finishing coat layer comprise the plant powder and the wood powder and are combined with the primer glue layer and the cover surface, so that a net knot-shaped coating is formed on the wall surface, and the purposes of improving the flexibility, saving energy and protecting the environment are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coatings and preparation methods thereof, and in particular to a cellulose environmentally friendly decorative material and a preparation method thereof. Background Art

[0002] Latex paint, textured paint, real stone paint, and artistic paint are all based on chemical emulsions of propylene and benzene, which also contain formaldehyde that can cause harm to the human body. Fillers are added to increase hardness. The fillers are mainly a mixture of stone powder, sand, chemical pigments, etc. The structure is too hard. When 1 to 3 zero cracks appear on the wall, the entire product surface will also crack. This is a problem that has not been solved in the paint industry for decades. The emulsion in the product formula is the main film-forming ingredient of the above four products. Since the emulsion is an oily substance, the remaining formula of 70% to 85% is water-based. The two are not highly compatible in structure. When the product humidity is 70% to 85%, the emulsion will form a protective film on the entire product surface. Because water and oil do not mix, there is no emulsion inside the entire product and between the wall. After the water evaporates, oil will only form on the surface of the product. The interior is too hard, with no tensile resistance or compatibility. Experiments have shown that the above products, after being completely dry, whether it is wall primer putty powder or talcum powder, or latex paint, real stone paint, texture paint, will become powder under the action of external force. After several years, some newly decorated house walls will have local surface cracks and finally fall off. Because the wall is very dry, it can be clearly observed at the location where the surface latex component falls off that the bottom primer material, putty, or talcum powder will form a dry powder, which completely loses all adhesion to the wall and the surface latex. In addition, the wall is damp and alkali-resistant, this situation will occur earlier, and the affected part will bubble and fall off, seriously affecting the decoration effect of the entire house. Furniture and equipment are all put away, which will cause a lot of trouble for maintenance in the later stage. As for most paint products currently on the market, they are generally chemical mixtures. Because they are compounds, many of the chemical substances they contain are harmful to the human body. In particular, formaldehyde is a carcinogen. Formaldehyde has a great impact on the upper respiratory tract and is also irritating to the eyes. People with sensitive skin may also develop allergies, even cancer, and endanger their lives in indoor environments containing formaldehyde.

[0003] The process of the prior art generally includes adding 107 or 108 glue to talcum powder. Putty powder comes with dry glue. Add appropriate amount of clean water as the wall base primer material, generally two or three times. After the primer is treated, it is polished with 280# or 360# sand. The surface is treated with latex paint by rolling or coating. Textured paint and real stone paint are directly scraped with putty powder or talcum powder for primer, and then coated or applied on the surface.

[0004] The above products are too hard, not soft, easy to crack, cold, not warm, and will turn white and fade over time. The emulsion is composed of propylene and benzene components, containing formaldehyde, which is harmful to the human body. Because each process is to wait for drying before the next construction, there is no good compatibility between putty powder and latex paint, texture paint, and real stone paint. It is easy to form a diaphragm layer between each process, which is easy to cause blistering and shedding. The emulsion component only forms a thin protective layer on the surface of the product, and the surface emulsion component, after drying, is a hard, brittle substance with no softness and no tensile resistance. It does not play a big role in the internal structure of the wall putty powder. Once 1 to 3 zero cracks appear on the wall, cracks will also appear on the surface. As the primer putty powder or talcum powder ages, the colloidal substance in its product structure will lose its adhesion to the wall and the surface emulsion component, and form the initial powder. Once the wall is alkali-reactive or damp, the affected parts will bubble and fall off. This will cause considerable trouble for later high-rise maintenance and home users. Even after the repair, the entire product is no longer a whole, and this problem will occur frequently in the future. The raw materials putty powder and talcum powder are both ground from stone, which are non-renewable resources. They cause damage and pollution to the earth's ecological resources and the living environment. During the entire construction process, the entire wall needs to be polished. The dust formed during the polishing process will cause respiratory and visual damage to the construction workers. Although there are similar wall grinders, the machine has extremely high requirements for the flatness of the entire wall and cannot be generally applied. After the wall is sanded, the entire wall is not treated, and the dust from sanding will leave a layer of dry powder on the wall, which has a great impact on the adhesion between latex paint and the entire wall. Even if a feather brush or other tools are used to deal with it, the effect is not good. In addition, after the latex paint dries, it can only form a protective film on the surface of the putty powder, which does not have good permeability, so there is a layer of interlayer phenomenon. These phenomena will bring problems to the later stage. At the same time, dust will also have a certain impact on air quality and living environment. The most important thing is to cause great harm to human health.

[0005] In view of this, this application is filed. Summary of the invention

[0006] The purpose of the present invention is to provide a cellulose environmentally friendly decorative material and a preparation method thereof, by setting the primer layer and the topcoat layer to include plant powder and wood powder, combining with the primer glue layer and the topcoat, forming a network-like coating on the wall surface, so as to solve the problems of poor quality and poor environmental protection of the coating in the prior art.

[0007] The present invention is implemented by the following technical scheme: An embodiment of the present invention provides a cellulose environmentally friendly decorative material, comprising a primer adhesive layer, a primer layer, a topcoat layer and a finishing layer which are sequentially stacked and connected, wherein the primer adhesive layer is used to be connected to a building wall surface;

[0008] Wherein, both the primer layer and the topcoat layer contain plant powder and wood powder.

[0009] Preferably, the topcoat layer is prepared from the following raw materials in parts by weight:

[0010] 55-70 parts of topcoat glue, 1-5 parts of polyaluminum dihydrogen phosphate, 3-10 parts of talcum powder, 1-5 parts of aluminum hydroxide, 3-10 parts of glass fiber powder, 5-15 parts of wood powder and 10-30 parts of plant powder.

[0011] Preferably, the primer layer is prepared by including the following raw materials in parts by weight:

[0012] 60-70 parts of primer glue, 2-8 parts of polyaluminum dihydrogen phosphate, 3-10 parts of talcum powder, 1-6 parts of aluminum hydroxide, 10-20 parts of wood powder, and 5-15 parts of plant powder.

[0013] Preferably, the raw materials for preparing the primer adhesive layer include 2 to 4 parts of waterproof glue and 0.8 to 1.2 parts of plant glue.

[0014] Preferably, the raw materials for preparing the topcoat layer include 1.5 to 2.5 parts of waterproof glue and 0.8 to 1.2 parts of plant glue.

[0015] In order to better solve the above problems, the embodiment of the present invention further provides a method for preparing a cellulose environmentally friendly decorative material, comprising the following steps:

[0016] S1: Primer glue layer: Mix waterproof glue and plant glue and apply them on the building wall to evaporate;

[0017] S2: When 60-80wt% of the water in the primer adhesive layer evaporates, a primer layer is applied on the primer adhesive layer;

[0018] S3: When 65-85wt% of the water in the primer layer evaporates, a topcoat layer is applied on the primer layer;

[0019] S4: When 70-90wt% of the water in the topcoat layer evaporates, scraping and pressing are performed;

[0020] S5: After the water content of the product in S4 evaporates, a finishing layer is applied on the topcoat layer, and after the water content of the finishing layer evaporates, the above-mentioned decorative material is obtained.

[0021] Preferably, the method for preparing the plant glue comprises the following steps:

[0022] Step 1: Mix water, flour (such as edible flour, plant flour), and crystal sugar, then heat to 80-100°C, continue stirring, and then cool;

[0023] Step 2: sequentially adding a mixture of sodium carboxymethyl cellulose, guar gum, soybean powder and water at room temperature to the mixed solution in step 1, then heating the mixture to perform gelatinization reaction to obtain a paste, and cooling the paste;

[0024] Step 3: adding an antibacterial and antifungal agent, sodium D-isoascorbate, to the cooled paste, and stirring to obtain plant glue;

[0025] The mass ratios of water, guar gum, sodium carboxymethyl cellulose, soybean powder, flour, crystal sugar, antibacterial and antifungal agent and sodium D-isoascorbate are 80-90: 0.5-2: 0.5-3: 0.5-2: 0.8-3: 1-4: 0.6-1.2: 0.5-1 respectively.

[0026] Preferably, the preparation method of the primer glue comprises mixing and stirring plant glue, natural emulsion (mainly rubber hydrocarbon), waterproof glue (mainly pure acrylic emulsion), fluorocarbon emulsion, silane coupling agent, glutinous rice grass liquid, antibacterial and mildewproof agent, and sodium D-isoascorbate to obtain the primer glue, and the weight parts are 40-50:5-15:15-25:5-12:3-10:5-13:0.5-1.5:0.3-1;

[0027] The preparation method of the topcoat glue comprises the following steps: mixing and stirring plant glue, natural emulsion, waterproof glue, fluorocarbon emulsion, silane coupling agent, glutinous rice grass liquid, polyaluminum dihydrogen phosphate, antibacterial and mildewproof agent, and D-sodium isoascorbate to obtain the topcoat glue, and the weight proportions are 40-60:6-14:10-22:1-7:2-8:7-17:3-10:0.5-1.2:0.3-0.8 respectively.

[0028] Preferably, the preparation process of the coating in the primer layer includes soaking plant powder and wood powder in a 15-25wt% ammonium polyphosphate solution, leaving it open for 24-48 hours, and then adding primer glue, polyaluminum dihydrogen phosphate, talcum powder, and aluminum hydroxide for stirring and mixing to obtain a primer layer coating.

[0029] Preferably, the preparation process of the coating material in the topcoat layer includes soaking plant powder and wood powder in an ammonium polyphosphate solution with a concentration of 15 to 25wt%, leaving it open for 15 to 35 hours, and then adding topcoat glue, polyaluminum dihydrogen phosphate, talcum powder, aluminum hydroxide, and glass fiber powder for stirring and mixing to obtain a topcoat layer coating material.

[0030] Compared with the prior art, the embodiments of the present invention have the following advantages and beneficial effects:

[0031] 1. The decorative material provided by the embodiment of the present invention includes a primer adhesive layer, a primer layer, a topcoat layer and a covering layer. The primer layer and the topcoat layer both contain plant powder and wood powder. Combined with the primer adhesive layer and the covering layer, it is not only soft but also environmentally friendly and energy-saving. The plant powder and wood powder can form a mesh structure, which not only increases the aesthetics of the building wall, but also increases the sound insulation performance. The primer adhesive layer has moisture-proof and tear-resistant functions. The covering layer can seal and protect the entire decorative material, enhance the durability, mildew resistance, isolation resistance, wear resistance, scrub resistance, acid and alkali resistance, oxidation resistance, corrosion resistance, waterproofness, etc. of the entire decorative material. The primer layer makes the decorative material and the building wall more mutually beneficial and connected, and can play a waterproof role. The topcoat layer has the effects of reinforcement and fire retardancy.

[0032] 2. In the preparation method provided by the present invention, each process retains the reserved humidity, so when the next process is constructed, there is good compatibility, connectivity and symbiosis, and there will be no isolation layer, bubbling or falling off. At the same time, plant glue is used to further improve the softness of the decorative material, and the waterproof glue has strong permeability, which can improve the waterproofness of the decorative material.

[0033] 3. In the preparation method of the embodiment of the present invention, even if 1 to 3 zero cracks appear on the wall, the decorative material will not crack, the protective strength is large, and the decorative effect is good. At the same time, there is no wall polishing process during the preparation or construction process, which will not harm the health of the construction workers, will not pollute the living environment, and will not affect the air quality.

[0034] In general, the embodiment of the present invention provides a cellulose environmentally friendly decorative material and a preparation method thereof, which forms a knotty coating on the wall surface by setting the primer layer and the topcoat layer to include plant powder and wood powder, and combining them with the primer glue layer and the topcoat, so as to achieve the purpose of improving softness, energy saving and environmental protection. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0036] Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] It should be noted that plant powder is made by grinding dried plants and generally contains the following main substances:

[0038] (1) Protein: The protein in plants usually becomes more concentrated after drying, so dried plants will contain a higher protein content.

[0039] (2) Cellulose: The cellulose in plants is usually not greatly affected after drying, so the dried plants still contain a high fiber content.

[0040] (3) Carbohydrates: Carbohydrates in plants usually become more concentrated after drying, so dried plants will also contain a higher carbohydrate content.

[0041] (4) Vitamins and minerals: The vitamins and minerals in plants will suffer a certain loss after drying, so the dried plants will contain less vitamins and minerals.

[0042] Wood powder is made by grinding wood materials after drying, and generally contains the following main substances:

[0043] (1) Cellulose is one of the most important components of wood. It is a linear polymer compound composed of many glucose molecules connected by β-1,4-glycosidic bonds. When wood is dried, cellulose will degrade to form some short-chain polysaccharides and monosaccharides, such as glucose, fructose and galactose.

[0044] (2) Hemicellulose is another important component of wood. It is a complex mixture of different polysaccharides. When wood is dried, hemicellulose will also degrade to form some short-chain polysaccharides and monosaccharides, such as xylose, arabinose and mannose.

[0045] (3) Lignin is one of the hardest components in wood. It is a three-dimensional polymer compound composed of a variety of different phenylpropane units connected by C-C chains. When wood is dried, the structure of lignin does not change significantly, but its chemical properties may change. For example, some functional groups in lignin may undergo oxidation or reduction reactions.

[0046] (4) In addition to cellulose, hemicellulose and lignin, wood also contains some other substances, such as resins, oils, tannins and pigments.

[0047] In the embodiment of the present invention, the decorative material is prepared by the recycled fusion of plant and wood gum, which can bring a healthy, green, environmentally friendly and original ecological indoor environment. Natural plants and wood have natural pigments, and can better reflect the colors of nature without adding any pigments. They are also superior in anti-oxidation and preventing the wall from fading.

[0048] Illustratively, an embodiment of the present invention provides a method for preparing a cellulose environmentally friendly decorative material. First, the base of the clear water wall is treated to ensure that the base is flat and solid. If there are cracks or depressions, they should be filled and repaired, and then the following steps are performed:

[0049] Step 1: Primer glue layer: Mix transparent waterproof glue and plant glue in a mass ratio of 3:1 and roll evenly on the wall. Brush the entire wall to completely and evenly cover the entire base surface. The primer glue layer is the base material for the entire wall, which can prevent the wall from being damp, alkali-induced, and the product surface from bubbling and falling off in the later stage.

[0050] Step 2: When 60-80wt% of the water in the primer adhesive layer evaporates, the primer coating material is scraped off in batches and applied on the primer adhesive layer for 2-3 times until the wall surface is smooth to obtain a primer layer;

[0051] Step 3: When 65-85wt% of the water in the primer layer evaporates, a topcoat layer is applied on the primer layer, i.e., the topcoat layer is sprayed or scraped 1-2 times;

[0052] Step 4: When 70-90wt% of the water in the topcoat layer evaporates, use a trowel to scrape and press the entire product wall to make it smooth and flat;

[0053] Step 5: After the moisture in the product evaporates, apply a finishing layer on the topcoat layer. After the moisture in the finishing layer evaporates, the decorative material is obtained, wherein the finishing paint is a mixture of waterproof glue and plant glue, and the mixing mass ratio is 2:1, and it can be sprayed or rolled.

[0054] The preparation method of plant glue is as follows: in a stirring container, water, flour and crystal sugar are added in sequence, the speed of the disperser is maintained at 200-500r / min, stirring is performed for 1-3min, and then heating is performed at 80-100 degrees, the speed of the disperser is maintained at 500-1000r / min, stirring is performed for 1-3min, and after cooling, sodium carboxymethyl cellulose and guar gum are added in sequence, and soybean powder is added in the form of a mixture of normal temperature water, heated for gelatinization, and then continued to be added, the speed of the disperser is maintained at 1000-3000r / min, and cooling and stirring is performed for 2-5min, and finally an antibacterial and mildew-proof agent (produced by Lvtai Environmental Protection Technology Co., Ltd.) and sodium D-isoascorbate are added, and the speed of the disperser is maintained at 300-600r / min, stirring is performed for 1-3min, and the plant glue is prepared. Among them, the mass part of water is 80 parts to 90 parts, the mass part of guar gum is 0.5 parts to 2 parts, the mass part of sodium carboxymethyl cellulose is 0.5 parts to 3 parts, the mass part of soybean powder is 0.5 parts to 2 parts, the mass part of flour is 0.8 parts to 3 parts, the mass part of crystal sugar is 1 parts to 4 parts, the mass part of antibacterial and mildewproof agent is 0.6 parts to 1.2 parts, and the mass part of sodium D-isoascorbate is 0.5 parts to 1 parts.

[0055] The preparation method of primer glue is as follows: 40 to 50 parts by weight of plant glue, 5 to 15 parts by weight of natural emulsion, 15 to 25 parts by weight of transparent strong waterproof glue (produced by Sichuan New Sanya Building Materials Technology Co., Ltd.), 5 to 12 parts by weight of fluorocarbon emulsion, 3 to 10 parts by weight of silane coupling agent, 5 to 13 parts by weight of glutinous rice grass liquid, 0.5 to 1.5 parts by weight of antibacterial and mildewproof agent, and 0.3 to 1 part by weight of D-sodium isoascorbate are sequentially added into a disperser, the speed of the disperser is maintained at 500 to 1000 r / min, and the primer glue is prepared by stirring for 3 to 5 minutes, wherein the latex molecules in the natural latex liquid can react with the silane coupling agent to form chemical bonds, so that the emulsion is cured to form a cured structure.

[0056] The guar gum and sodium carboxymethyl cellulose mentioned above can increase the viscosity of the solution and form a gel in water, making the glue more viscous. At the same time, the guar gum and sodium carboxymethyl cellulose can increase the stability of the solution, making the glue less likely to stratify. The protein and sugar in the flour can undergo a Maillard reaction when heated to produce brown substances and aroma. The silane coupling agent reacts with the starch and protein in the flour to form chemical bonds, thereby enhancing the strength and stability of the flour in water and making the glue less likely to deteriorate.

[0057] The preparation method of the topcoat glue is as follows: 40 to 60 parts by weight of plant glue, 6 to 14 parts by weight of natural emulsion, 10 to 22 parts by weight of transparent strong waterproof glue (produced by Sichuan New Sanya Building Materials Technology Co., Ltd.), 1 to 7 parts by weight of fluorocarbon emulsion, 2 to 8 parts by weight of silane coupling agent, 7 to 17 parts by weight of glutinous rice grass liquid, 3 to 10 parts by weight of polyaluminum dihydrogen phosphate, 0.5 to 1.2 parts by weight of antibacterial and mildewproof agent, and 0.3 to 0.8 parts by weight of D-sodium isoascorbate are added in a disperser in sequence, the speed of the disperser is maintained at 500 to 1000 r / min, and stirring is performed for 3 to 5 minutes to prepare the topcoat glue.

[0058] The preparation method of the primer coating material comprises the following steps: taking 10 to 20 parts by weight of wood powder with a fineness of 80 to 120 meshes and 5 to 15 parts by weight of plant powder with a fineness of 60 to 100 meshes, and then soaking them in a 20wt% ammonium polyphosphate solution for 36 hours, and when the water evaporates to a humidity of 10 to 30wt%, adding 60 to 70 parts by weight of primer glue, and then adding the whole into a disperser, and then successively adding 2 to 8 parts by weight of polyaluminum dihydrogen phosphate, 3 to 10 parts by weight of talc powder with a fineness of 200 meshes, and 1 to 6 parts by weight of aluminum hydroxide into the disperser, keeping the speed of the disperser at 300 to 800 r / min, stirring for 3 to 5 minutes, and then packaging and sealing to obtain the primer coating material.

[0059] The preparation method of the topcoat coating material comprises the following steps: taking 5 to 15 parts by weight of wood powder with a fineness of 80 to 120 meshes and 10 to 30 parts by weight of plant powder with a fineness of 60 to 100 meshes, and then soaking them in a 20wt% ammonium polyphosphate solution for 24 hours. When the water evaporates to a humidity of 10 to 30wt%, adding 55 to 70 parts by weight of topcoat glue, and then adding the whole into a disperser. Then, 3 to 10 parts by weight of polyaluminum dihydrogen phosphate, 3 to 10 parts by weight of talc with a fineness of 200 meshes, 1 to 5 parts by weight of aluminum hydroxide, and 3 to 10 parts by weight of alkali-free reinforced, toughened and hardened glass fiber powder (with a fineness of 400 meshes) are added into the disperser in sequence. The speed of the disperser is kept at 300 to 600 r / min, and the mixture is stirred for 3 to 6 minutes. The mixture can be packaged and sealed to obtain the topcoat coating material.

[0060] In the above preparation process, guar gum and sodium carboxymethyl cellulose can form a gel, flour and bean powder can form a paste, plant powder and wood powder can enhance the strength and stability of the structural system, natural latex can form a rubber-like substance, and silane coupling agent can enhance the bonding force between various components. It should be noted that the main component of natural latex is rubber hydrocarbon, which can enhance the wear resistance and corrosion resistance of decorative materials. At the same time, the surface tension of rubber hydrocarbon molecular chains is low, which can prevent water and moisture from entering the interior of the material.

[0061] Ammonium polyphosphate is a commonly used inorganic flame retardant, which can form a stable carbon layer during the combustion process, thereby preventing the propagation and spread of flames. Polyaluminum dihydrogen phosphate is a new type of inorganic flame retardant, which can release a large amount of water vapor during the combustion process, thereby reducing the temperature and oxygen concentration in the combustion area, achieving a fire-retardant effect. The simultaneous use of ammonium polyphosphate and polyaluminum dihydrogen phosphate can give play to their respective advantages, form a synergistic effect, and improve the fire-retardant effect. Preferably, when the environmentally friendly decorative material of the embodiment of the present invention is constructed on the wall, the construction temperature can be controlled at 20 to 30 degrees. Within this temperature range, the surface film forming time is 20 to 40 minutes.

[0062] Example 1

[0063] The embodiment of the present invention provides a method for preparing an environmentally friendly cellulose decorative material. First, the base of the clear water wall is processed to ensure that the base is flat and solid. If there are cracks or depressions, they should be filled and repaired. Then, the following steps are performed:

[0064] Step 1: Primer glue layer: Mix transparent waterproof glue and plant glue in a mass ratio of 3:1 and roll evenly on the wall. Brush the entire wall to completely and evenly cover the entire base surface. The primer glue layer is the base material for the entire wall, which can prevent the wall from being damp, alkali-induced, and the product surface from bubbling and falling off in the later stage.

[0065] Step 2: When 70wt% of the water in the primer glue layer evaporates, scrape the primer layer coating material in batches and apply it on the primer glue layer, apply it twice until the wall surface is flat, and obtain the primer layer;

[0066] Step 3: When 80wt% of the water in the primer layer evaporates, a topcoat layer is applied on the primer layer, i.e., the topcoat layer is sprayed or scraped twice;

[0067] Step 4: When 80wt% of the water in the topcoat layer evaporates, use a trowel to scrape and press the entire product wall to make it smooth and flat;

[0068] Step 5: After the moisture in the product evaporates, apply a finishing layer on the topcoat layer. After the moisture in the finishing layer evaporates, the decorative material is obtained, wherein the finishing paint is a mixture of waterproof glue and plant glue, and the mixing mass ratio is 2:1, and it can be sprayed or rolled.

[0069] The preparation method of plant glue: in a stirred container, water, flour, crystal sugar are added in sequence, the dispersion machine speed is kept at 400r / min, stirred for 2min, then heated to 90 degrees, the dispersion machine speed is kept at 800r / min, stirred for 2min, carboxymethyl cellulose sodium and guar gum are added in sequence after cooling, and soybean powder is added in the form of a normal temperature water mixture, heated for gelatinization, and then continued to be added, the dispersion machine speed is kept at 2000r / min, cooled and stirred for 4min, and finally antibacterial and mildewproof agent (produced by Lvtai Environmental Protection Technology Co., Ltd.) and D-isoascorbic acid sodium are added, with a dispersion machine speed of 500r / min, stirred for 2min, and plant glue is obtained. Wherein, the mass parts of water are 85 parts, the mass parts of guar gum are 1 part, the mass parts of carboxymethyl cellulose sodium are 2 parts, the mass parts of soybean powder are 1 part, the mass parts of flour are 2 parts, the mass parts of crystal sugar are 3 parts, the mass parts of antibacterial and mildewproof agent are 0.8 parts, and the mass parts of D-isoascorbic acid sodium are 0.7 parts.

[0070] The preparation method of primer glue is as follows: 45 parts by weight of plant glue, 10 parts by weight of natural emulsion, 20 parts by weight of transparent strong waterproof glue (produced by Sichuan New Sanya Building Materials Technology Co., Ltd.), 8 parts by weight of fluorocarbon emulsion, 6 parts by weight of silane coupling agent, 8 parts by weight of glutinous rice grass liquid, 1 part by weight of antibacterial and mildewproof agent, and 2 parts by weight of D-sodium isoascorbate are added in a disperser in sequence, the speed of the disperser is maintained at 800 r / min, and the primer glue is prepared by stirring for 4 minutes. The latex molecules in the natural latex liquid can react with the silane coupling agent to form chemical bonds, so that the emulsion is cured to form a cured structure.

[0071] Preparation method of topcoat glue: add 50 parts by weight of plant glue, 10 parts by weight of natural emulsion, 15 parts by weight of transparent strong waterproof glue (produced by Sichuan New Sanya Building Materials Technology Co., Ltd.), 4 parts by weight of fluorocarbon emulsion, 5 parts by weight of silane coupling agent, 10 parts by weight of glutinous rice grass liquid, 6 parts by weight of polyaluminum dihydrogen phosphate, 0.9 parts by weight of antibacterial and mildewproof agent, and 0.5 parts by weight of D-sodium isoascorbate in a disperser in sequence, keep the disperser speed at 800 r / min, and stir for 4 minutes to prepare the topcoat glue.

[0072] The preparation method of the primer coating material is as follows: 15 parts by weight of wood powder with a fineness of 100 meshes and 10 parts by weight of plant powder with a fineness of 80 meshes are mixed, and then immersed in a 20wt% ammonium polyphosphate solution for 36 hours. When the water evaporates to a humidity of 20wt%, 65 parts by weight of primer glue are added, and then the whole is added to a disperser. Then, 5 parts by weight of polyaluminum dihydrogen phosphate, 6 parts by weight of talc powder with a fineness of 200 meshes, and 4 parts by weight of aluminum hydroxide are added to the disperser in turn. The speed of the disperser is maintained at 500r / min, and stirring is carried out for 4 minutes. Then, the mixture can be packaged and sealed to obtain the primer coating material.

[0073] The preparation method of the topcoat coating material is as follows: 10 parts by weight of wood powder with a fineness of 100 meshes and 20 parts by weight of plant powder with a fineness of 80 meshes are mixed, and then immersed in a 20wt% ammonium polyphosphate solution for 24 hours. When the water evaporates to a humidity of 20wt%, 60 parts by weight of topcoat glue are added, and then the whole is added to a disperser. Then, 6 parts by weight of polyaluminum dihydrogen phosphate, 7 parts by weight of talc with a fineness of 200 meshes, 3 parts by weight of aluminum hydroxide, and 6 parts by weight of alkali-free reinforced, toughened and hardened glass fiber powder (fineness of 400 meshes) are added to the disperser in turn. The speed of the disperser is maintained at 500r / min, and stirred for 5 minutes, and then packaged and sealed to obtain the topcoat coating material.

[0074] The decorative material prepared by the preparation method provided in Example 1 of the present invention improves the service life and effect of the entire wall surface. No interlayer is produced in each process. The interior and surface of the entire product are a whole, and can withstand 1 to 3 zero gaps in the wall and keep the product from cracking.

[0075] The decorative material of Example 1 of the present invention is prepared on a PVC board, which can withstand a bending angle of 30 degrees without cracking, and can withstand a bending angle of 180 degrees when made on newspapers.

[0076] In the absence of a topcoat, the primer layer and the topcoat layer can withstand a 20wt% sulfuric acid solution and will not cause blistering, loosening of decorative materials, or powdering within half a month of immersion, and have high structural compatibility and corrosion resistance.

[0077] The covering layer has high permeability, water resistance, acid and alkali resistance, mildew resistance, high strength and elasticity, and can enhance the adhesion between the entire product's network-like internal structural system and the entire wall.

[0078] Pure natural plants and wood powder have a high natural texture surface effect. The entire wall can smell the original scent of plants and wood. It can achieve zero release of formaldehyde and harmful poisons, and will not cause any harm or pollution to the human body and the environment. The entire wall feels warm and visually warm, making people feel comfortable physically and mentally.

[0079] After gelatinization, soybean powder becomes a good adhesive. It not only has strong adhesion but also has no pollution. It is suitable for coating after combining with water and can maintain strong adhesion after drying.

[0080] Regardless of the season, in the same room, because this product has the characteristics of both plant fiber and wood fiber, it has good softness and compatibility, and also has the functions of thermal expansion and contraction and heat storage. The tensile strength, crack resistance and thermal insulation effect are greatly improved. At the same time, it also has the function of regulating indoor humidity. When the indoor humidity is high, the fiber in the product will absorb a certain amount of water vapor. When the indoor temperature is dry, the water vapor absorbed in the fiber will diffuse into the room.

[0081] The performance of the primer coating material prepared in Example 1 was tested, and the results are shown in Table 1. The performance of the topcoat coating material was tested, and the results are shown in Table 2.

[0082] Table 1: Primer coating material performance test results

[0083] Test items Technical requirements Measured value Status in container GB / T9756-2018 No lumps, even after stirring Low temperature stability GB / T9756-2018 No deterioration after 3 cycles Coating appearance GB / T9756-2018 normal Alkali resistance GB / T9756-2018 No abnormality in 24 hours Anti-alkali GB / T9756-2018 No abnormality in 48 hours

[0084] Table 2: Topcoat coating material performance test results

[0085] Test items Technical requirements unit Measured value Status in container GB / T9756-2018 / No lumps, even after stirring Low temperature stability GB / T9756-2018 / No deterioration after 3 cycles Coating appearance GB / T9756-2018 / normal Alkali resistance GB / T9756-2018 / No abnormality in 24 hours Anti-scrubbing GB / T9756-2018 Second-rate >350

[0086] The decorative material prepared in Example 1 was subjected to a performance test, wherein the test method is as follows:

[0087] Solid content: Add appropriate amount of water to the primer coating and topcoat coating respectively, mix them to make the coating completely dissolved, measure the specific gravity of the mixture with a hydrometer, and determine it by calculating the difference between the specific gravity of the mixture and the specific gravity of water.

[0088] Surface drying time: Take 30cm*40cm PVC board, make primer and topcoat samples respectively, place them at a constant temperature of 20 degrees, and the result is obtained.

[0089] Waterproofness: The finished product is made on a clean glass plate, and then placed in a sealed container. Water is added to the container to make the water level higher than the coating surface, and then 0.3 MPa of air pressure is applied to the container for 50 minutes. No bubbles or water seepage occur.

[0090] Softness: Bending test, the finished product is made on a 30cm*40cm PVC sample board and on rubber, and can withstand 30 and 180 degree bending respectively without cracking or peeling. Freeze resistance test, put it in a freezer at minus 30 degrees for 24 hours, and there is no crack or breakage.

[0091] Fire resistance: The finished product is made on a plain water wall, and a flamethrower is used to burn the same part with a strong flame. In the end, only carbonization will be formed. After leaving the fire, it will not burn again.

[0092] Permeability of primer glue layer and topcoat: Apply the primer glue layer and topcoat on two glass plates respectively, then place a standard filter paper on each glue surface, and observe the speed and degree of wetting of the filter paper.

[0093] The test results are shown in Table 3 below:

[0094] Table 3: Test results of decorative material performance

[0095]

[0096]

[0097] Comparative Example 1: A method for preparing an environmentally friendly cellulose decorative material is provided. The difference from Example 1 is that no plant powder is added during the preparation of the primer coating material and the topcoat coating material, and the other steps remain unchanged.

[0098] Example 2: A method for preparing an environmentally friendly cellulose decorative material is provided. The difference from Example 1 is that in the preparation process of the primer coating, 25 parts by weight of wood powder are added, and in the preparation process of the topcoat coating, 10 parts by weight of wood powder are added, and the other steps remain unchanged.

[0099] Example 3: A method for preparing a cellulose environmentally friendly decorative material is provided. The difference from Example 1 is that the mass ratio of the waterproof glue and the plant glue in the topcoat is 1:3, and the other steps remain unchanged.

[0100] Example 4: A method for preparing an environmentally friendly cellulose decorative material is provided. The difference from Example 1 is that during the preparation of the primer coating material, the added primer glue is replaced with plant glue, and the other steps remain unchanged.

[0101] Example 5: A method for preparing an environmentally friendly cellulose decorative material is provided. The difference from Example 1 is that during the preparation of the primer coating material, 1 part by weight of polyaluminum dihydrogen phosphate is added.

[0102] The decorative materials prepared in Comparative Example 1 and Examples 2-5 were subjected to performance testing, and the testing method was the same as that of Example 1. The test results obtained were compared with those of the decorative materials of Example 1, and the comparison is shown in Table 4 below:

[0103] Table 4

[0104]

[0105]

[0106] As can be seen from Table 4, by comparing the test results of Comparative Example 1 and Example 1, it can be seen that when plant powder is not added during the preparation process, obvious cracks will appear in the material. Although wood powder has a certain flexibility, wood fiber is a relatively hard substance. It has poor flexibility when used alone in the preparation of decorative materials. The flexibility of plant powder is far superior to that of wood powder fiber, which can improve the flexibility, tensile resistance, connectivity and symbiosis of the product.

[0107] From the comparison between Example 2 and Example 1, it can be seen that if the amount of wood powder added to the primer coating is too high, the compatibility and compatibility between the topcoat layer and the primer layer will be reduced, resulting in slight cracks in the entire decorative material. Therefore, the relative proportion of the amount of plant powder and wood powder is very important. If the amount of plant powder is too high, the decorative material of the embodiment of the present invention will be too soft and insufficient in strength, resulting in easy deformation and insufficient durability.

[0108] From the comparison between Example 3 and Example 1, it can be seen that the waterproof glue of the topcoat has a waterproof effect. If the usage is too low, the waterproofness, fire resistance and corrosion resistance of the decorative material will be reduced.

[0109] By comparing Example 4 with Example 1, it can be seen that the overall effect of the decorative material obtained by preparing the primer glue obtained by configuring the plant glue alone will be better than the decorative material using only the plant glue.

[0110] By comparing Example 5 with Example 1, it can be seen that reducing the amount of polyaluminum dihydrogen phosphate can significantly reduce the fire resistance of the decorative material.

[0111] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A cellulose environmentally friendly decorative material, characterized in that: It includes sequentially stacking and connecting a primer adhesive layer, a primer layer, a topcoat layer and a finishing layer, wherein the primer adhesive layer is used to be connected to a building wall surface; Wherein, both the primer layer and the topcoat layer contain plant powder and wood powder.

2. The environmentally friendly cellulose decorative material according to claim 1, characterized in that: The topcoat layer is prepared from the following raw materials in parts by weight: 55-70 parts of topcoat glue, 1-5 parts of polyaluminum dihydrogen phosphate, 3-10 parts of talcum powder, 1-5 parts of aluminum hydroxide, 3-10 parts of glass fiber powder, 5-15 parts of wood powder and 10-30 parts of plant powder.

3. The environmentally friendly cellulose decorative material according to claim 2, characterized in that: The primer layer is prepared from the following raw materials in parts by weight: 60-70 parts of primer glue, 2-8 parts of polyaluminum dihydrogen phosphate, 3-10 parts of talcum powder, 1-6 parts of aluminum hydroxide, 10-20 parts of wood powder, and 5-15 parts of plant powder.

4. The environmentally friendly cellulose decorative material according to claim 3, characterized in that: The raw materials for preparing the primer adhesive layer include 2 to 4 parts of waterproof glue and 0.8 to 1.2 parts of plant glue.

5. The environmentally friendly cellulose decorative material according to claim 4, characterized in that: The raw materials for preparing the cover layer include 1.5 to 2.5 parts of waterproof glue and 0.8 to 1.2 parts of plant glue.

6. A method for preparing an environmentally friendly cellulose decorative material, characterized in that: The following steps are involved: S1: Primer glue layer: Mix waterproof glue and plant glue and apply them on the building wall to evaporate; S2: When 60-80wt% of the water in the primer adhesive layer evaporates, a primer layer is applied on the primer adhesive layer; S3: When 65-85wt% of the water in the primer layer evaporates, a topcoat layer is applied on the primer layer; S4: When 70-90wt% of the water in the topcoat layer evaporates, scraping and pressing are performed; S5: After the water content of the product in S4 evaporates, a finishing layer is applied on the topcoat layer, and after the water content of the finishing layer evaporates, the decorative material according to any one of claims 1 to 5 is obtained.

7. The method for preparing an environmentally friendly cellulose decorative material according to claim 6, characterized in that: The preparation method of the plant glue comprises the following steps: Step 1: Mix water, flour and rock sugar, then heat to 80-100℃, continue stirring and cool; Step 2: sequentially adding a mixture of sodium carboxymethyl cellulose, guar gum, soybean powder and water at room temperature to the mixed solution in step 1, then heating the mixture to perform gelatinization reaction to obtain a paste, and cooling the paste; Step 3: adding an antibacterial and antifungal agent, sodium D-isoascorbate, to the cooled paste, and stirring to obtain plant glue; The mass ratios of water, guar gum, sodium carboxymethyl cellulose, soybean powder, flour, crystal sugar, antibacterial and antifungal agent and sodium D-isoascorbate are 80-90: 0.5-2: 0.5-3: 0.5-2: 0.8-3: 1-4: 0.6-1.2: 0.5-1 respectively.

8. The method for preparing an environmentally friendly cellulose decorative material according to claim 7, characterized in that: The preparation method of the primer glue comprises mixing and stirring plant glue, natural emulsion, waterproof glue, fluorocarbon emulsion, silane coupling agent, glutinous rice grass liquid, antibacterial and mildewproof agent, and sodium D-isoascorbate to obtain the primer glue, and the weight parts are 40-50:5-15:15-25:5-12:3-10:5-13:0.5-1.5:0.3-1; The preparation method of the topcoat glue comprises the following steps: mixing and stirring plant glue, natural emulsion, waterproof glue, fluorocarbon emulsion, silane coupling agent, glutinous rice grass liquid, polyaluminum dihydrogen phosphate, antibacterial and mildewproof agent, and D-sodium isoascorbate to obtain the topcoat glue, and the weight proportions are 40-60:6-14:10-22:1-7:2-8:7-17:3-10:0.5-1.2:0.3-0.8 respectively.

9. The method for preparing an environmentally friendly cellulose decorative material according to claim 6, characterized in that: The preparation process of the coating material in the primer layer includes soaking plant powder and wood powder in a polyphosphate ammonium solution with a concentration of 15-25wt%, leaving it open for 24-48 hours, and then adding primer glue, polyaluminum dihydrogen phosphate, talcum powder, and aluminum hydroxide for stirring and mixing to obtain the primer layer coating material.

10. The method for preparing an environmentally friendly cellulose decorative material according to claim 6, characterized in that: The preparation process of the coating material in the topcoat layer includes soaking plant powder and wood powder in an ammonium polyphosphate solution with a concentration of 15-25wt%, leaving it open for 15-35 hours, and then adding topcoat glue, polyaluminum dihydrogen phosphate, talcum powder, aluminum hydroxide, and glass fiber powder for stirring and mixing to obtain the topcoat layer coating material.

Citation Information

Patent Citations

  • Environment-friendly glue and production process thereof

    CN110903781A

  • High-strength environment-friendly adhesive and preparation method thereof

    CN113337226A

  • Layer structure is scribbled to high abrasion elastomer outer wall emulsion paint