C-grade solvent-free organic silicon impregnating varnish and preparation method thereof
By using vinyl methylphenyl silicone resin and hydrogen-containing methylphenyl silicone resin in silicone impregnated paint to perform the hydrosilica addition reaction, and adjust the molar ratio of structural units, combined with the secondary reaction method, the silicone was solved The impregnated paint has defects in temperature resistance, achieving higher mechanical strength and heat resistance.
Patent Information
- Application Number
- CN202411137201.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing silicone impregnated paint has defects in temperature resistance and ideal insulation properties and mechanical strength, resulting in unsatisfactory practical application results.
Using vinyl methylphenyl silicone resin and hydrogen-containing methylphenyl silicone resin as the main components, a highly crosslinked network structure was formed through the hydrogen silicon addition reaction, and the molar ratio of each structural unit was adjusted, combined with the secondary reaction method. , prepare C-grade solvent-free silicone impregnated paint to improve mechanical strength, heat resistance and insulation properties.
The mechanical strength, heat resistance and insulation properties of silicone impregnated paint have been significantly improved, the defects in related technologies have been overcome, and the actual application effect of the product has been improved.
Smart Images

Figure BDA0004999751470000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of chemical materials, and more specifically, to a Class C solvent-free organic silicon impregnation varnish and a preparation method thereof. Background Art
[0002] Electrical insulation impregnation resin is one of the main insulating materials used in electrical products. It is an indispensable insulating material in AC and DC motors, impregnated dry-type transformers, power transformers and other equipment. In the 1950s and 1960s, electrical insulation impregnation resins generally used solvent paints, which generally contained about 50% organic solvents and required multiple impregnations during use. There were many problems such as long impregnation process time, serious environmental pollution, and poor production safety. In the 1970s, as a substitute for traditional solvent paints, solvent-free paints began to be vigorously promoted. Most solvent-free paints are styrene-based, which generally contain 30% to 40% styrene. The main function is to solve the problem of dryness in the winding, which can effectively reduce the number of impregnations and improve production efficiency. However, the disadvantage is that there are still a lot of volatiles during baking and the storage life is short. By the 1980s, foreign countries began to steadily promote the vacuum (pressure) impregnation process under the premise of pursuing the reliability, heat resistance and environmental resistance of electrical products, and launched a new generation of low-volatile impregnation resins. This new impregnation resin is characterized by not releasing a large amount of volatiles during the impregnation and heat curing process, good stability, fast curing, and internal filling of up to 98%. In contrast, the development of domestic electrical insulation impregnation resins is still insufficient. In China, there are limited varieties of electrical insulation impregnation paints with heat resistance grade H or above. For decades, solvent-based silicone paints have been the main products, and there are relatively few solvent-free impregnation resin products.
[0003] The main component of silicone impregnation varnish is polyorganosiloxane with a highly cross-linked network structure, which can be divided into condensation type and addition type according to the cross-linking curing method. Condensation type silicone impregnation varnish uses silicone resin prepolymer containing Si-OH, Si-OR and other groups as raw materials, which are further condensed and cross-linked into solid products under the action of catalysts or heating; addition type silicone impregnation varnish uses polysiloxane containing Si-Vi bonds and siloxane containing Si-H bonds as raw materials, which are cross-linked by silane hydrogen addition reaction under the action of catalysts. Compared with condensation type silicone impregnation varnish, addition type silicone impregnation varnish has the advantages of no organic solvent, no by-products during curing, small shrinkage, deep curing, short production cycle and high efficiency.
[0004] A Chinese patent document with publication number CN108329474A discloses a one-component addition-type silicone impregnation paint organic silicone resin and its preparation method and application. The one-component addition-type silicone impregnation paint organic silicone resin is prepared by using an alkoxysilane mixture as a raw material through hydrolysis-condensation reaction, end-capping reaction and post-treatment. The invention prepares a one-component addition-type silicone impregnation paint organic silicone resin with a narrow molecular weight distribution and extremely low residual hydrogen chloride content through the above process. The one-component addition-type silicone impregnation paint prepared with the organic silicone resin as a raw material has an extremely low volatilization amount at 200°C / 1h.
[0005] Another example is a Chinese patent document with publication number CN107641466A, which discloses a solvent-free silicone impregnation varnish and a preparation method thereof, by introducing a structural formula of SiR n X 4-n The silicone monomer B can reserve silicon vinyl or silicon hydrogen groups in the molecular chain of the silicone prepolymer, and can form a silicone solvent-free impregnation varnish through silicon hydrogen addition reaction during the later curing. The impregnation varnish prepared by the invention does not release low molecular weight substances when curing into a film, does not affect the electrical performance, is pollution-free, and also has good electrical and mechanical properties.
[0006] With respect to the above-mentioned related technologies, the inventors believe that the silicone impregnating varnish in the related technologies has the defect of low temperature resistance grade, and it is difficult to have both ideal insulation performance and mechanical strength, resulting in unsatisfactory actual application effect of the product. Summary of the invention
[0007] The organic silicon impregnation varnish in the related art has a low temperature resistance grade and is difficult to have both ideal insulation performance and mechanical strength, and the actual application effect is not ideal. In order to improve this defect, the present application provides a Class C solvent-free organic silicon impregnation varnish and a preparation method thereof.
[0008] In a first aspect, the present application provides a Class C solvent-free organosilicon impregnation varnish, which adopts the following technical scheme: a Class C solvent-free organosilicon impregnation varnish, wherein the organosilicon impregnation varnish is made of the following raw materials in parts by weight: 1 part of vinyl methyl phenyl silicone resin, 1-1.2 parts of hydrogenated methyl phenyl silicone resin, 0.01-0.05 parts of catalyst, and 0.01-0.05 parts of inhibitor; the general structural formula of the vinyl methyl phenyl silicone resin is (MeSi0 1.5 ) m (Me2Si0) n (PhSi0 1.5 ) x (Ph2Si0) y (Me2ViSiO 0.5 ) z, m:n:x:y:z=(0.3-0.45):(0.1-0.2):(0.2-0.35):(0.1-0.2):(0.15-0.25); the general structural formula of the hydrogen-containing methylphenyl silicone resin is (MeSi0 1.5 ) M (Me2Si0) N (PhSi0 1.5 ) X (Ph2Si0) Y (Me2HSiO 0.5 ) Z , M:N:X:Y:Z=(0.25-0.35):(0.1-0.2):(0.3-0.4):(0.1-0.2):(0.25-0.35).
[0009] By adopting the above technical solution, the present application preferably selects vinyl methyl phenyl silicone resin and hydrogen-containing methyl phenyl silicone resin as the main components of the silicone impregnation varnish. The vinyl group in the vinyl methyl phenyl silicone resin and the Si-H group in the hydrogen-containing methyl phenyl silicone resin can undergo a cross-linking reaction under the joint control of a catalyst and an inhibitor to form a polyorganosiloxane with a highly cross-linked network structure. At the same time, the present application also defines the chain segment composition of the vinyl methyl phenyl silicone resin and the hydrogen-containing methyl phenyl silicone resin. By adjusting the MeSi0 1.5 Structural unit, Me2Si0 structural unit, PhSi0 1.5 The molar ratio between the structural units and the Ph2Si0 structural units keeps the viscosity of the resin within an appropriate range, while the mechanical strength, heat resistance and insulation properties of the silicone impregnating varnish are greatly improved, thereby overcoming the defects in the relevant technology and improving the actual application effect of the silicone impregnating varnish products.
[0010] Preferably, the Me2HSiO 0.5 The structural unit is provided by a dimethylhydrogensiloxane monomer, wherein the dimethylhydrogensiloxane monomer is one of dimethylethoxysilane and tetramethyldisiloxane; the Me2ViSiO 0.5 The structural unit is provided by a dimethylvinylsiloxane monomer, and the dimethylvinylsiloxane monomer is one of dimethylvinylmethoxysilane, dimethylvinylethoxysilane, and tetramethyldivinyldisiloxane.
[0011] By adopting the above technical solution, the present application preferably provides Me2HSiO 0.5 Structural unit and Me2ViSiO 0.5 The siloxane monomer type of the structural unit is represented by MeSi0 1.5 Structural unit, Me2Si0 structural unit, PhSi01.5 The combination of structural units and Ph2Si0 structural units, on this basis, the silicone impregnation varnish products prepared by selecting the above-mentioned types of monomers can have good mechanical strength, heat resistance and insulation properties.
[0012] Preferably, the catalyst is a platinum catalyst, and the platinum catalyst is one of chloroplatinic acid-isopropanol solution or platinum-divinyltetramethyldisiloxane complex.
[0013] By adopting the above technical solution, the present application optimizes the specific type of catalyst, and the above two platinum catalysts can catalyze the hydrosilylation reaction.
[0014] Preferably, the inhibitor is an organic compound containing an alkynyl group, and the organic compound containing an alkynyl group is one of 1-ethynylcyclohexanol, 3,5-dimethyl-3-hexyn-1-ol, and 3-methyl-1-butyn-3-ol.
[0015] By adopting the above technical scheme, the present application optimizes the specific type of inhibitor. The selection of the above type of inhibitor can realize the control of the hydrosilylation reaction together with the catalyst, thereby making the silicone impregnation paint product have good mechanical strength, heat resistance and insulation properties.
[0016] In a second aspect, the present application provides a method for preparing a Class C solvent-free silicone impregnation varnish, using the following technical solution.
[0017] A method for preparing a Class C solvent-free silicone impregnating varnish comprises the following steps: (1) mixing a siloxane monomer, a solvent and an inorganic acid, heating the mixture for reaction, cooling the product to room temperature, extracting the mixture to obtain an organic phase, adding an inorganic base to the organic phase under heating conditions, reacting the mixture for a period of time, cooling the organic phase, adding a neutralizing agent and a solvent, washing the organic phase with water and removing low boiling points, and obtaining a vinyl methyl phenyl silicone resin; (2) mixing a siloxane monomer, a solvent, and an inorganic acid, heating the mixture to react, cooling the product to room temperature, extracting the mixture to obtain an organic phase, adding an inorganic acid to the organic phase under heating conditions, reacting the mixture for a period of time, adding a solvent, washing the mixture with water, and removing low boiling points to obtain a hydrogen-containing methyl phenyl silicone resin; (3) The vinylmethylphenyl silicone resin obtained in step (1) and the hydrogenated methylphenyl silicone resin obtained in step (2), a catalyst and an inhibitor are mixed according to a proportion, and after stirring and reacting, a Class C solvent-free silicone impregnation varnish is obtained.
[0018] By adopting the above technical scheme, the present application uses a secondary reaction method to process vinylmethylphenyl silicone resin and hydrogen-containing methylphenyl silicone resin, and obtains two silicone resins containing vinyl and Si-H groups, and then makes these two silicone resins undergo a silylation reaction to obtain a Class C solvent-free silicone impregnation varnish. Specifically, in the preparation step of vinylmethylphenyl silicone resin, the method of the present application first uses an inorganic acid for a hydrolysis condensation reaction, and then continues to use an inorganic base for a hydrolysis condensation reaction; in the preparation method of hydrogen-containing methylphenyl silicone resin, first uses an inorganic acid for a hydrolysis condensation reaction, and then continues to use an inorganic acid for a hydrolysis condensation reaction; this can greatly reduce the content of unreacted hydroxyl groups in the resin structure, thereby further improving the mechanical strength, heat resistance and insulation properties of the resin.
[0019] Preferably, in step (1) and step (2) of the method, the inorganic acid mixed with the siloxane monomer and the solvent is a hydrochloric acid solution.
[0020] By adopting the above technical solution, the present application optimizes the specific type of inorganic acid and realizes the preparation of vinyl methyl phenyl silicone resin and hydrogen-containing methyl phenyl silicone resin.
[0021] Preferably, in step (2) of the method, the inorganic acid added to the organic phase is concentrated sulfuric acid.
[0022] By adopting the above technical solution, the present application optimizes the specific type of inorganic acid and realizes the preparation of hydrogen-containing methylphenyl silicone resin.
[0023] Preferably, in step (1) and step (2) of the method, the extractant is selected from one of toluene, xylene and petroleum ether, and the solvent used is one of methanol, ethanol, ethyl acetate and butyl acetate.
[0024] By adopting the above technical solution, the present application optimizes the specific types of extractants and solvents, and realizes the preparation of vinyl methyl phenyl silicone resin and hydrogen-containing methyl phenyl silicone resin.
[0025] Preferably, in step (1) of the method, the inorganic base used is one of sodium hydroxide and potassium hydroxide.
[0026] By adopting the above technical solution, the present application optimizes the specific type of inorganic base and realizes the preparation of vinylmethylphenyl silicone resin.
[0027] Preferably, in step (1) of the method, the neutralizing agent used is concentrated hydrochloric acid or concentrated sulfuric acid.
[0028] By adopting the above technical solution, the present application optimizes the specific type of neutralizer and realizes the preparation of vinylmethylphenyl silicone resin.
[0029] In summary, this application has the following beneficial effects: 1. The present application preferably uses vinyl methyl phenyl silicone resin and hydrogen-containing methyl phenyl silicone resin as the main components of the silicone impregnation varnish, and uses the hydrosilylation reaction to form a polyorganosiloxane with a highly cross-linked network structure. At the same time, the present application adjusts the molar ratio between the structural units so that the viscosity of the resin is maintained within a suitable range, while the mechanical strength, heat resistance and insulation properties of the silicone impregnation varnish are greatly improved, thereby overcoming the defects in the relevant technology and improving the actual application effect of the silicone impregnation varnish product.
[0030] 2. The method of the present application uses a secondary reaction method to process vinyl methyl phenyl silicone resin and hydrogen-containing methyl phenyl silicone resin to obtain two silicone resins containing vinyl and Si-H groups, and then the two silicone resins undergo a hydrosilylation reaction to obtain a Class C solvent-free silicone impregnation varnish. By controlling the synthesis conditions of vinyl methyl phenyl silicone resin and hydrogen-containing methyl phenyl silicone resin, the content of unreacted hydroxyl groups in the resin structure can be greatly reduced, thereby further improving the mechanical strength, heat resistance and insulation properties of the resin. DETAILED DESCRIPTION
[0031] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially. Example
[0032] In the examples and comparative examples of the present application, the concentrated sulfuric acid used is 98 wt % concentrated sulfuric acid, and the concentrated hydrochloric acid is 38 wt % concentrated hydrochloric acid.
[0033] Examples 1-8 The following description is given by taking Example 1 as an example.
[0034] Example 1 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and dimethylvinylethoxysilane are added into a reactor at a molar ratio of 0.35:0.1:0.35:0.1:0.25, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 50° C., a 15 wt % hydrochloric acid solution at a mass fraction of 5% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 115° C., the acid drive treatment is carried out for 60 min, sodium hydroxide at a mass fraction of 0.2% of the total monomers is added, the reaction is carried out for 4 h, the reaction is cooled to room temperature, concentrated hydrochloric acid and ethanol are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extractant used is toluene; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.3:0.1:0.35:0.1:0.35, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 40° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 5% of the total monomers is added, the reaction is carried out for 6 h, ethanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.1:0.03:0.03 and physically blend them; in this step, the catalyst is chloroplatinic acid-isopropanol solution, and the inhibitor is 1-ethynylcyclohexanol.
[0035] Example 2 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane and dimethylvinylmethoxysilane are added into a reactor at a molar ratio of 0.35:0.1:0.35:0.1:0.25, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 55° C., a 15 wt % hydrochloric acid solution at a mass fraction of 5% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 5 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 120° C., the acid drive treatment is carried out for 60 min, sodium hydroxide at a mass fraction of 0.2% of the total monomers is added, the reaction is carried out for 3 h, the reaction is cooled to room temperature, concentrated hydrochloric acid and ethanol are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extraction agent used is xylene; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.3:0.1:0.35:0.1:0.35, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 40° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 5% of the total monomers is added, the reaction is carried out for 6 h, ethanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.1:0.03:0.03 and physically blend them; in this step, the catalyst is chloroplatinic acid-isopropanol solution, and the inhibitor is 1-ethynylcyclohexanol.
[0036] Example 3 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltrimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane and tetramethyldivinyldisiloxane are added into a reactor at a molar ratio of 0.3:0.15:0.35:0.1:0.15, ethanol is added into the reactor at a mass fraction of 15% of the total monomers, the temperature is raised to 50° C., a 20 wt % hydrochloric acid solution at a mass fraction of 5% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 80° C., the reaction is carried out for 4 h, the reaction is cooled to room temperature, toluene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 110° C., the acid drive treatment is carried out for 60 min, sodium hydroxide at a mass fraction of 0.3% of the total monomers is added, the reaction is carried out for 3 h, the reaction is cooled to room temperature, concentrated sulfuric acid and ethanol are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extraction agent used is petroleum ether; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.35:0.1:0.35:0.15:0.35, ethanol is added into the reactor at a mass fraction of 15% of the total monomers, the temperature is raised to 45° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 80° C., the reaction is carried out for 5 h, the reaction is cooled to room temperature, toluene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 6% of the total monomers is added, the reaction is carried out for 5 h, ethanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.08:0.02:0.02 and physically blend them; in this step, the catalyst is chloroplatinic acid-isopropanol solution, and the inhibitor is 3,5-dimethyl-3-hexyn-1-ol.
[0037] Example 4 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltriethoxysilane, dimethyldimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane and tetramethyldivinyldisiloxane are added into a reactor at a molar ratio of 0.3:0.15:0.35:0.1:0.2, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 50° C., a 15 wt % hydrochloric acid solution at a mass fraction of 5% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 85° C., the reaction is carried out for 4 h, the reaction is cooled to room temperature, toluene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 120° C., the acid drive treatment is carried out for 30 min, sodium hydroxide at a mass fraction of 0.3% of the total monomers is added, the reaction is carried out for 3 h, the reaction is cooled to room temperature, concentrated sulfuric acid and methanol are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extractant used is toluene; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltriethoxysilane, dimethyldimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.3:0.1:0.35:0.2:0.35, ethanol is added into the reactor at a mass fraction of 15% of the total monomers, the temperature is raised to 45° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, toluene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 6% of the total monomers is added, the reaction is carried out for 5 h, ethanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.08:0.02:0.02 and physically blend them; in this step, the catalyst is chloroplatinic acid-isopropanol solution, and the inhibitor is 3,5-dimethyl-3-hexyn-1-ol.
[0038] Example 5 This embodiment provides a Class C solvent-free organic silicon impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane and dimethylvinylethoxysilane are added into a reactor at a molar ratio of 0.45:0.15:0.2:0.1:0.25, methanol is added at a mass fraction of 10% of the total monomers into the reactor, the temperature is raised to 50° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 5 h, the temperature is further raised to 80° C., the reaction is carried out for 4 h, the reaction is cooled to room temperature, petroleum ether is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 110° C., the acid drive treatment is carried out for 60 min, potassium hydroxide at a mass fraction of 0.3% of the total monomers is added, the reaction is carried out for 4 h, the reaction is cooled to room temperature, concentrated hydrochloric acid and ethyl acetate are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extraction agent used is xylene; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane and dimethylethoxysilane are added into a reactor at a molar ratio of 0.35:0.1:0.3:0.15:0.25, methanol is added at a mass fraction of 10% of the total monomers into the reactor, the temperature is raised to 45° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 85° C., the reaction is carried out for 5 h, the reaction is cooled to room temperature, petroleum ether is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 6% of the total monomers is added, the reaction is carried out for 4 h, methanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.2:0.05:0.05 and physically blend them; in this step, the catalyst is platinum-divinyltetramethyldisiloxane complex, and the inhibitor is 3,5-dimethyl-3-hexyn-1-ol.
[0039] Example 6 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltriethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and dimethylvinylmethoxysilane are added into a reactor at a molar ratio of 0.45:0.15:0.3:0.1:0.25, methanol is added at a mass fraction of 15% of the total monomers into the reactor, the temperature is raised to 55° C., a 20 wt % hydrochloric acid solution at a mass fraction of 5% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 85° C., the reaction is carried out for 5 h, the reaction is cooled to room temperature, petroleum ether is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 120° C., the acid drive treatment is carried out for 30 min, potassium hydroxide at a mass fraction of 0.1% of the total monomers is added, the reaction is carried out for 4 h, the reaction is cooled to room temperature, concentrated hydrochloric acid and butyl acetate are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extraction agent used is petroleum ether; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltriethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.35:0.1:0.3:0.15:0.3, methanol at a mass fraction of 15% of the total monomers is added into the reactor, the temperature is raised to 40° C., a 20 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 80° C., the reaction is carried out for 4 h, the reaction is cooled to room temperature, petroleum ether is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 4% of the total monomers is added, the reaction is carried out for 6 h, methanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), a catalyst and an inhibitor in a mass ratio of 1:1.15:0.05:0.05 and physically blend them; in this step, the catalyst is a platinum-divinyltetramethyldisiloxane complex, and the inhibitor is 3-methyl-1-butyn-3-ol.
[0040] Example 7 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltrimethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane and tetramethyldivinyldisiloxane are added into a reactor at a molar ratio of 0.4:0.2:0.35:0.2:0.25, butyl acetate is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 55° C., a 15 wt % hydrochloric acid solution at a mass fraction of 6% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 85° C., the reaction is carried out for 5 h, the reaction is cooled to room temperature, toluene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 115° C., the acid drive treatment is carried out for 45 min, potassium hydroxide at a mass fraction of 0.2% of the total monomers is added, the reaction is carried out for 2 h, the reaction is cooled to room temperature, concentrated sulfuric acid and butyl acetate are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extractant used is toluene; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane and dimethylethoxysilane are added into a reactor at a molar ratio of 0.25:0.15:0.35:0.1:0.35, butyl acetate is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 40° C., a 15 wt % hydrochloric acid solution at a mass fraction of 5% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 80° C., the reaction is carried out for 4 h, the reaction is cooled to room temperature, toluene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 4% of the total monomers is added, the reaction is carried out for 6 h, butyl acetate is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), a catalyst and an inhibitor in a mass ratio of 1:1.05:0.01:0.01 and physically blend them; in this step, the catalyst is a platinum-divinyltetramethyldisiloxane complex, and the inhibitor is 3-methyl-1-butyn-3-ol.
[0041] Example 8 This embodiment provides a Class C solvent-free silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltriethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane and tetramethyldivinyldisiloxane are added into a reactor at a molar ratio of 0.4:0.15:0.35:0.15:0.25, butyl acetate is added into the reactor at a mass fraction of 15% of the total monomers, the temperature is raised to 50° C., a 20 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 4 h, the temperature is further raised to 80° C., the reaction is carried out for 4 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 120° C., the acid drive treatment is carried out for 30 min, potassium hydroxide at a mass fraction of 0.1% of the total monomers is added, the reaction is carried out for 4 h, the reaction is cooled to room temperature, concentrated sulfuric acid and butyl acetate are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; in this step, the extractant used is xylene; (2) Synthesis of hydrogenated methylphenyl silicone resin: Methyltriethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.25:0.2:0.4:0.1:0.35, butyl acetate is added into the reactor at a mass fraction of 15% of the total monomers, the temperature is raised to 45° C., a 20 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 85° C., the reaction is carried out for 5 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 5% of the total monomers is added, the reaction is carried out for 5 h, butyl acetate is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), a catalyst and an inhibitor in a mass ratio of 1:1:0.01:0.01 and physically blend them; in this step, the catalyst is a platinum-divinyltetramethyldisiloxane complex, and the inhibitor is 3-methyl-1-butyn-3-ol.
[0042] Comparative Example Comparative Example 1 The organosilicon impregnating varnish was prepared with reference to Example 1 of Chinese Patent Publication No. CN108329474A.
[0043] Comparative Example 2 The organosilicon impregnating varnish was prepared with reference to Example 1 of Chinese Patent Publication No. CN107641466A.
[0044] Comparative Example 3 This comparative example provides a silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinyl methyl phenyl silicone resin: methyl trimethoxysilane, dimethyl dimethoxysilane, phenyl trimethoxysilane, diphenyl dimethoxysilane, and dimethyl vinyl ethoxysilane are added into a reactor at a molar ratio of 0.25:0.1:0.4:0.1:0.25, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 50° C., a 15 wt % hydrochloric acid solution is added dropwise at a mass fraction of 5% of the total monomers, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinyl methyl phenyl silicone resin; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.3:0.1:0.35:0.1:0.35, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 40° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinylmethylphenyl silicone resin obtained in step (1), the hydrogenated methylphenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.1:0.03:0.03 and physically blend.
[0045] Comparative Example 4 This comparative example provides a silicone impregnating varnish, which is prepared according to the following method: (1) Synthesis of vinylmethylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and dimethylvinylethoxysilane are added into a reactor at a molar ratio of 0.25:0.25:0.4:0.25:0.2, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 50° C., a 15 wt % hydrochloric acid solution is added dropwise at a mass fraction of 5% of the total monomers, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, the temperature is raised to 115° C., the acid drive treatment is carried out for 60 min, sodium hydroxide is added at a mass fraction of 0.2% of the total monomers, the reaction is carried out for 4 h, the reaction is cooled to room temperature, concentrated hydrochloric acid and ethanol are added, the reaction solution is washed with water until it is neutral, and low boiling points are removed under vacuum conditions to obtain vinylmethylphenyl silicone resin; (2) Synthesis of hydrogenated methylphenyl silicone resin: methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane and tetramethyldisiloxane are added into a reactor at a molar ratio of 0.4:0.25:0.25:0.25:0.2, ethanol is added into the reactor at a mass fraction of 10% of the total monomers, the temperature is raised to 40° C., a 15 wt % hydrochloric acid solution at a mass fraction of 4% of the total monomers is added dropwise, the reaction is carried out for 3 h, the temperature is further raised to 80° C., the reaction is carried out for 6 h, the reaction is cooled to room temperature, xylene is added, and after extraction and separation, the organic phase is added into the reactor, concentrated sulfuric acid at a mass fraction of 5% of the total monomers is added, the reaction is carried out for 6 h, ethanol is added, the reaction solution is washed with water until it is neutral, and low-boiling substances are removed under vacuum conditions to obtain hydrogenated methylphenyl silicone resin; (3) Preparation of Class C solvent-free silicone impregnation varnish: Add the vinyl methyl phenyl silicone resin obtained in step (1), the hydrogenated methyl phenyl silicone resin obtained in step (2), the catalyst and the inhibitor in a mass ratio of 1:1.1:0.02:0.01 and physically blend.
[0046] Performance testing methods According to GB / T 15022.2-2017 Resin-based active composites for electrical insulation Part 2: Test methods, the performance of the silicone impregnating varnishes of each embodiment and comparative example was tested, and the test items included: viscosity, Shore D hardness, cured volatile matter, electrical strength, volume resistivity, dielectric loss factor, adhesion, tensile strength, flexural strength, and heat resistance. The results are shown in Table 1.
[0047] Table 1 Combining Examples 1-8 and Comparative Examples 1-4 with Table 1, it can be seen that the mechanical properties, insulation properties and heat resistance of the organosilicon impregnating varnishes prepared in the examples are significantly better than those of the organosilicon impregnating varnishes prepared in the comparative examples while ensuring appropriate viscosity. The main disadvantage of the organosilicon impregnating varnish of Comparative Example 1 is that the temperature resistance level is not high and there is no good mechanical strength, while the main disadvantage of the organosilicon impregnating varnish of Comparative Example 2 is that the temperature resistance level is not high and its insulation performance is not very good. In Comparative Example 3, because the secondary reaction method was not adopted and only one acid-catalyzed reaction was carried out, Si-OH groups would still remain in the silicone resin chain. During the curing process of the silicone impregnating varnish, these unreacted Si-OH groups would continue to undergo condensation reactions, and the resulting small molecules would seriously affect the curing process, causing the mechanical properties, insulation properties and heat resistance of the silicone impregnating varnish to be greatly reduced. In Comparative Example 4, because the molar ratio between the structural units was outside the range specified in the present application, the side groups in these structural units failed to exert their synergistic effect to the greatest extent, resulting in a decrease in the mechanical properties, insulation properties and heat resistance of the silicone impregnating varnish of Comparative Example 4.
[0048] The above embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments of the present application without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A Class C solvent-free silicone impregnating varnish, characterized in that: The organic silicon impregnation varnish is made of the following raw materials in parts by weight: 1 part of vinyl methyl phenyl silicone resin, 1-1.2 parts of hydrogen-containing methyl phenyl silicone resin, 0.01-0.05 parts of catalyst, and 0.01-0.05 parts of inhibitor; the general structural formula of the vinyl methyl phenyl silicone resin is (MeSi0 1.5 ) m (Me2Si0) n (PhSi0 1.5 ) x (Ph2Si0) y (Me2ViSiO 0.5 ) z , m:n:x:y:z=(0.3-0.45):(0.1-0.2):(0.2-0.35):(0.1-0.2):(0.15-0.25); the general structural formula of the hydrogen-containing methylphenyl silicone resin is (MeSi0 1.5 ) M (Me2Si0) N (PhSi0 1.5 ) X (Ph2Si0) Y (Me2HSiO 0.5 ) Z , M:N:X:Y:Z=(0.25-0.35):(0.1-0.2):(0.3-0.4):(0.1-0.2):(0.25-0.35).
2. The C-class solvent-free silicone impregnation varnish according to claim 1, characterized in that: The Me2HSiO 0.5 The structural unit is provided by a dimethylhydrogensiloxane monomer, wherein the dimethylhydrogensiloxane monomer is one of dimethylethoxysilane and tetramethyldisiloxane; the Me2ViSiO 0.5 The structural unit is provided by a dimethylvinylsiloxane monomer, and the dimethylvinylsiloxane monomer is one of dimethylvinylmethoxysilane, dimethylvinylethoxysilane, and tetramethyldivinyldisiloxane.
3. The C-class solvent-free silicone impregnating varnish according to claim 1, characterized in that: The catalyst is a platinum catalyst, and the platinum catalyst is one of chloroplatinic acid-isopropanol solution or platinum-divinyltetramethyldisiloxane complex.
4. The C-class solvent-free silicone impregnating varnish according to claim 1, characterized in that: The inhibitor is an organic compound containing an alkynyl group, and the organic compound containing an alkynyl group is one of 1-ethynylcyclohexanol, 3,5-dimethyl-3-hexyn-1-ol, and 3-methyl-1-butyn-3-ol.
5. The method for preparing a Class C solvent-free silicone impregnating varnish according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Mixing a siloxane monomer, a solvent and an inorganic acid, heating the mixture to react, cooling the product to room temperature, extracting the organic phase, adding an inorganic base to the organic phase under heating conditions, reacting the mixture for a period of time, cooling the organic phase, adding a neutralizing agent and a solvent, washing the organic phase with water and removing the low boiling point, and obtaining a vinyl methyl phenyl silicone resin; (2) mixing a siloxane monomer, a solvent and an inorganic acid, heating the mixture for reaction, cooling the product to room temperature, extracting the organic phase, adding an inorganic acid to the organic phase under heating conditions, reacting the mixture for a period of time, adding a solvent, washing the mixture with water and removing low boiling points to obtain a hydrogen-containing methyl phenyl silicone resin; (3) The vinyl methyl phenyl silicone resin obtained in step (1), the hydrogenated methyl phenyl silicone resin obtained in step (2), a catalyst and an inhibitor are mixed according to a proportion, and after stirring and reacting, a Class C solvent-free organic silicone impregnation varnish is obtained.
6. The method for preparing a Class C solvent-free silicone impregnating varnish according to claim 5, characterized in that: In step (1) and step (2) of the method, the inorganic acid mixed with the siloxane monomer and the solvent is a hydrochloric acid solution.
7. The method for preparing a Class C solvent-free silicone impregnating varnish according to claim 6, characterized in that: In step (2) of the method, the inorganic acid added to the organic phase is concentrated sulfuric acid.
8. The method for preparing a Class C solvent-free silicone impregnating varnish according to claim 5, characterized in that: In step (1) and step (2) of the method, the extractant is selected from one of toluene, xylene and petroleum ether, and the solvent used is one of methanol, ethanol, ethyl acetate and butyl acetate.
9. The method for preparing a Class C solvent-free silicone impregnating varnish according to claim 5, characterized in that: In step (1) of the method, the inorganic base used is one of sodium hydroxide and potassium hydroxide.
10. The method for preparing a Class C solvent-free silicone impregnating varnish according to claim 5, characterized in that: In step (1) of the method, the neutralizing agent used is concentrated hydrochloric acid or concentrated sulfuric acid.
Citation Information
Patent Citations
One part solventless conformal coatings
CA2064989A1
Solvent-free nuclear motor coil impregnating varnish and preparation method thereof
CN103421424A
Preparation method for organic silicon impregnating varnish
CN105295720A
Primer for condensed organic silicon pressure-sensitive adhesive and preparation method of primer
CN117025095A
Organic silicon coating
WO2017024693A1