Preparation method of natural rubber modified emulsion glue

By preparing natural rubber modified emulsion glue, the existing adhesives have poor water resistance and prone to mildew deterioration, and high viscosity and strength adhesives are achieved, meeting the high stability needs of cartons and providing safe and environmentally friendly solutions.

CN118909564APending Publication Date: 2024-11-08ZHEJIANG GREAT SHENGDA PACKING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411119781.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing environmentally friendly adhesives have poor water resistance and are prone to mold and deterioration during industrial use, resulting in a decrease in adhesive performance and it is difficult to meet the high strength and stability needs of cartons.

Method used

The preparation method of natural rubber modified emulsion glue is adopted, and the vulcanization reaction and dilution treatment are carried out by preparing natural rubber emulsion, casein solution, NF solution, KOH solution, S dispersion, ZDC dispersion, ZnO dispersion and starch paste solution. Form a natural rubber modified emulsion glue with high viscosity and good adhesive strength.

Benefits of technology

It realizes an adhesive with high viscosity, strength and water resistance, ensures the edge pressure strength and stability of the carton, avoids the problem of mold and deterioration of the adhesive, and provides a safe and environmentally friendly solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909564A_ABST
    Figure CN118909564A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of natural rubber modified emulsion glue, which comprises the following steps: adding 100 parts of natural rubber emulsion, 0.5 part of 10% casein solution, 2.0 parts of 10% NF solution, 4.0 parts of 10% KOH solution, 1.5 parts of 50% S dispersion, 0.5 part of 50% ZDC dispersion and 0.5 part of 40% ZnO dispersion into a beaker according to the proportion, heating to 40-60 DEG C, and carrying out vulcanization reaction at the stirring speed of 300-330 r / min to obtain the natural rubber modified emulsion glue. And adding water to dilute the pre-vulcanized natural rubber latex, adding the starch paste solution, continuously stirring and reacting at 40 DEG C for 10-50 minutes, and cooling at room temperature to obtain the rubber latex. The natural rubber latex is used as a main raw material, is non-toxic, environment-friendly and safe to use, can effectively overcome the defects of low strength, poor water resistance, easiness in mildewing and deterioration, poor stability and the like of an existing carton packaging adhesive, and has wide popularization and application values.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a packaging carton adhesive, and more particularly to a preparation method and application of a natural rubber modified latex adhesive. Background Art

[0002] With the rapid development of e-commerce and the implementation of the plastic restriction order, express cartons are considered to have a strong alternative to traditional non-degradable plastic bag products, and also conform to the sustainable development concept of "paper instead of plastic". As an important material for bonding cartons, the quality of adhesives directly affects the edge compression strength of cartons, and the adhesive performance also affects the moisture return and moisture absorption of cartons. At present, the environmentally friendly adhesives that have entered industrial use are mainly based on starch, which is derived from edible raw materials such as corn, wheat, sweet potatoes, potatoes and mung beans. Although they have the advantages of no pollution and low cost, they compete with people for food. At the same time, because starch is hydrophilic, it has poor water resistance, is easy to mold and deteriorate, and has poor stability during industrial use, resulting in a decrease in bonding performance. Therefore, the development of new adhesives with high bonding strength, excellent water resistance / stability, safety and environmental protection has become the key to the recycling of cartons. Summary of the invention

[0003] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0004] The purpose of the present invention is to provide a natural rubber modified latex adhesive which is green and environmentally friendly, has strong bonding strength, excellent water resistance and stability, and is used for gluing packaging cartons.

[0005] In order to achieve these objects and other advantages according to the present invention, a method for preparing a natural rubber modified latex rubber is provided, which is prepared from the following raw materials in parts by weight: 100 parts of natural rubber latex, 0.5 parts of 10% casein solution, 2.0 parts of 10% NF solution, 4.0 parts of 10% KOH solution, 1.5 parts of 50% S dispersion, 0.5 parts of 50% ZDC dispersion, 0.5 parts of 40% ZnO dispersion, and 10 to 80 parts of starch paste solution;

[0006] The preparation method of the natural rubber modified latex comprises the following steps:

[0007] Step 1, preparing the 10% casein solution: weighing the ingredients according to 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of water, adding casein, borax and ammonia water in sequence at a stirring speed of 300-330 rpm, keeping the temperature below 50° C., stirring while heating until the ingredients are completely dissolved;

[0008] Step 2, preparing the 10% NF solution: adding 10 parts of the diffusion agent NF and 90 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the NF is completely dissolved, and cooling at room temperature for later use;

[0009] Step 3, preparing the 10% KOH solution: adding 10 parts of stabilizer KOH and 90 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the KOH is completely dissolved, and cooling to room temperature for later use;

[0010] Step 4, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use;

[0011] Step 5, preparing the 50% ZDC dispersion: grinding ZDC powder in a mortar for later use; adding 50 parts of accelerator ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use;

[0012] Step 6, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use;

[0013] Step 7, preparing the starch paste solution: adding starch and 95 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the starch is dissolved, gelatinizing at 70° C. for 30 minutes, and cooling at room temperature for later use;

[0014] Step eight, preparing a pre-vulcanized natural rubber latex: adding 100 parts of the natural rubber latex, 0.5 parts of the 10% casein solution, 2.0 parts of the 10% NF solution, 4.0 parts of the 10% KOH solution, 1.5 parts of the 50% S dispersion, 0.5 parts of the 50% ZDC dispersion and 0.5 parts of the 40% ZnO dispersion into a beaker according to a proportion, heating to 40-60° C., and performing a vulcanization reaction at a stirring speed of 300-330 rpm for 20-60 minutes;

[0015] Step nine, preparing natural rubber modified latex rubber: dilute the pre-vulcanized natural rubber latex obtained in step eight with water, then add the starch paste solution to the diluted pre-vulcanized natural rubber latex, continue stirring and reacting at 40° C. for 10 to 50 minutes, and cool to room temperature.

[0016] Preferably, the weight portion of starch in the starch paste solution is 5%.

[0017] Preferably, the vulcanization reaction time in step eight is 40 minutes and the vulcanization reaction temperature is 40°C.

[0018] Preferably, the stirring reaction time in step nine is 30 minutes.

[0019] Preferably, the starch in step seven is one or more of corn starch, wheat starch, tapioca starch and potato starch.

[0020] The present invention includes at least the following beneficial effects: the present invention uses natural rubber latex as the main raw material, is non-toxic, environmentally friendly, safe to use, and can effectively solve the shortcomings of existing carton packaging adhesives such as low strength, poor water resistance, easy mold and deterioration, poor stability, etc., and has wide promotion and application value.

[0021] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a method for preparing a natural rubber modified latex. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0024] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0025] Step 1, preparing the 10% casein solution: weighing the ingredients according to 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of water, adding casein, borax and ammonia water in sequence at a stirring speed of 300-330 rpm, keeping the temperature below 50° C., stirring while heating until the ingredients are completely dissolved;

[0026] Step 2, preparing the 10% NF solution: adding 10 parts of the diffusion agent NF and 90 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the NF is completely dissolved, and cooling at room temperature for later use;

[0027] Step 3, preparing the 10% KOH solution: adding 10 parts of stabilizer KOH and 90 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the KOH is completely dissolved, and cooling to room temperature for later use;

[0028] Step 4, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use;

[0029] Step 5, preparing the 50% ZDC dispersion: grinding ZDC powder in a mortar for later use; adding 50 parts of accelerator ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use;

[0030] Step 6, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use;

[0031] Step 7, preparing the starch paste solution: adding starch and 95 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the starch is dissolved, gelatinizing at 70° C. for 30 minutes, and cooling at room temperature for later use;

[0032] Step eight, preparing a pre-vulcanized natural rubber latex: adding 100 parts of the natural rubber latex, 0.5 parts of the 10% casein solution, 2.0 parts of the 10% NF solution, 4.0 parts of the 10% KOH solution, 1.5 parts of the 50% S dispersion, 0.5 parts of the 50% ZDC dispersion and 0.5 parts of the 40% ZnO dispersion into a beaker according to a proportion, heating to 40° C., and performing a vulcanization reaction at a stirring speed of 300-330 rpm for 40 minutes;

[0033] Step nine, preparing natural rubber modified latex rubber: dilute the pre-vulcanized natural rubber latex obtained in step eight with water, then add the starch paste solution to the diluted pre-vulcanized natural rubber latex, continue stirring and reacting at 40° C. for 30 minutes, and cool to room temperature.

[0034] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0035] As described above, the natural rubber modified latex glue prepared by the present invention has been tested to have a viscosity of 700-2000 mpa·s and a bonding strength of 5.88-24.49 N. After bonding, the adhesive was immersed in water for 5 days, and no debonding occurred at the bonding point, which reflects excellent water resistance and stability. The present invention uses natural rubber latex as the main raw material, is non-toxic, environmentally friendly, safe to use, and can effectively solve the shortcomings of existing carton packaging adhesives such as low strength, poor water resistance, easy mold and deterioration, poor stability, etc., and has a wide range of promotion and application value.

[0036] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and the embodiments. It can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily realized. Therefore, without departing from the general concept defined by the claims and equivalent scope, the present invention is not limited to the specific details and the illustrations shown and described here.

Claims

1. A method for preparing a natural rubber modified latex, characterized in that: The invention is prepared from the following raw materials in parts by weight: 100 parts of natural rubber latex, 0.5 parts of 10% casein solution, 2.0 parts of 10% NF solution, 4.0 parts of 10% KOH solution, 1.5 parts of 50% S dispersion, 0.5 parts of 50% ZDC dispersion, 0.5 parts of 40% ZnO dispersion, and 10-80 parts of starch paste solution; The preparation method of the natural rubber modified latex comprises the following steps: Step 1, preparing the 10% casein solution: weighing the ingredients according to 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of water, adding casein, borax and ammonia water in sequence at a stirring speed of 300-330 rpm, keeping the temperature below 50° C., stirring while heating until the ingredients are completely dissolved; Step 2, preparing the 10% NF solution: adding 10 parts of the diffusion agent NF and 90 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the NF is completely dissolved, and cooling at room temperature for later use; Step 3, preparing the 10% KOH solution: adding 10 parts of stabilizer KOH and 90 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the KOH is completely dissolved, and cooling to room temperature for later use; Step 4, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use; Step 5, preparing the 50% ZDC dispersion: grinding ZDC powder in a mortar for later use; adding 50 parts of accelerator ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use; Step 6, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water into a beaker, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and leaving it for more than 12 hours before use; Step 7, preparing the starch paste solution: adding starch and 95 parts of soft water into a beaker, stirring at a speed of 300-330 rpm until the starch is dissolved, gelatinizing at 70° C. for 30 minutes, and cooling at room temperature for later use; Step eight, preparing a pre-vulcanized natural rubber latex: adding 100 parts of the natural rubber latex, 0.5 parts of the 10% casein solution, 2.0 parts of the 10% NF solution, 4.0 parts of the 10% KOH solution, 1.5 parts of the 50% S dispersion, 0.5 parts of the 50% ZDC dispersion and 0.5 parts of the 40% ZnO dispersion into a beaker according to a proportion, heating to 40-60° C., and performing a vulcanization reaction at a stirring speed of 300-330 rpm for 20-60 minutes; Step nine, preparing natural rubber modified latex rubber: dilute the pre-vulcanized natural rubber latex obtained in step eight with water, then add the starch paste solution to the diluted pre-vulcanized natural rubber latex, continue stirring and reacting at 40° C. for 10 to 50 minutes, and cool to room temperature.

2. The method for preparing the natural rubber modified latex according to claim 1, wherein: The weight portion of starch in the starch paste solution is 5%.

3. The method for preparing the natural rubber modified latex according to claim 1, wherein: The vulcanization reaction time in step eight is 40 minutes, and the vulcanization reaction temperature is 40°C.

4. The method for preparing the natural rubber modified latex according to claim 1, wherein: The stirring reaction time in step nine is 30 minutes.

5. The method for preparing the natural rubber modified latex according to claim 1, characterized in that: The starch in step seven is one or more of corn starch, wheat starch, tapioca starch and potato starch.