Adhesive applied to aerogel covered hot-pressed film and preparation method of adhesive

By combining SKYBON saturated polyester ES-50 with Wanhua toluene diisocyanate TD-80 and Toyofang saturated polyester GK780, combined with aluminum hypophosphate OP935 and BYK-302, a kind of can be prepared in The adhesive with high peel strength, good flame retardancy and excellent pressure leakage current resistance after rapid thermal pressing at 110°C under exposed conditions has solved many of the shortcomings in the prior art. question.

CN118909579APending Publication Date: 2024-11-08GUANGXI ANXIN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989066.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing adhesive cannot be stored in 35℃ for at least 3 months under exposed conditions. At the same time, the peel strength is insufficient after rapid hot pressing at 110℃ at low temperature, and the flame retardant VTM-0, and the peel strength of glue to glue 35℃ is ≤0.2 The requirement for current ≤1mA when the voltage-tolerant leakage current is 2700V.

Method used

SKYBON saturated polyester ES-50 and Wanhua toluene diisocyanate TD-80, combined with Toyobosa saturated polyester GK780 and aluminum hypophosphate OP935, add BYK-302, and pass specific formula ratios and process steps. Prepare adhesives to improve peel strength, temperature resistance and flame retardant effect, and dissolve resin through xylene to improve permeability.

Benefits of technology

It has achieved peeling strength ≥1.31N/mm after storage at 35℃ for ≥3 months, and rapid thermal pressing at 110℃ at low temperatures, flame retardant VTM-0, glue-to-glue peeling strength ≤0.06N/mm and pressure-retardant leak-resistant Performance of current ≤1mA when current DC is 2700V.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958359720000051
    Figure BDA0004958359720000051
  • Figure BDA0004958359720000062
    Figure BDA0004958359720000062
  • Figure BDA0004958359720000071
    Figure BDA0004958359720000071
Patent Text Reader

Abstract

The invention relates to the field of adhesives, and discloses an adhesive applied to an aerogel covered hot-pressed film and a preparation method of the adhesive, and the adhesive comprises the following components by mass: 31-37% of SKYBON saturated polyester ES-500; 6%-8% of Dongyao saturated polyester GK780; 22% of aluminum hypophosphite OP935; 0.5 to 0.7 percent of Wanhua toluene diisocynate (TD-80); 0.08% of a BYK-302 (BYK-302) leveling agent; after the SKYBON saturated polyester ES-500 and the Wanhua toluene diisocynate TD-80 react, the peeling strength is provided; the Oriental polyester GK780 provides peel strength after reacting with Wanhua toluene diisocynate TD-80, and in addition, the softening point of the Oriental polyester GK780 is slightly higher than that of the SKYBON saturated polyester ES-500, so that the peel strength of the adhesive to the adhesive at 35 DEG C can be reduced; the adhesive disclosed by the invention can jointly realize the following five points: 1, the adhesive can be stored at 35 DEG C for at least 3 months under an exposed condition; 2, the peel strength is greater than or equal to 0.8 N / mm after the low temperature is 110 DEG C and rapid thermal compression bonding is carried out for 15S; 3, the flame retardance is VTM-0; 4, the peeling strength of the adhesive at 35 DEG C is less than or equal to 0.2 N / mm; and 5, withstand voltage leakage current: when the direct current is 2700V, the current is less than or equal to 1mA.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesives, in particular to an adhesive used for aerogel-covered hot-pressed film and a preparation method thereof. Background Art

[0002] Aerogel is a material with excellent thermal insulation properties, but its brittleness and mechanical strength limitations require certain methods to strengthen and protect it in practical applications. Covering aerogel on a hot-pressed film is a common solution, and adhesives play a key role in this process.

[0003] Existing adhesives cannot achieve the following 5 points together:

[0004] 1. Store at 35℃ for at least 3 months under bare conditions;

[0005] 2. Low temperature 110℃, 15S rapid hot pressing after peeling strength ≥0.8N / mm;

[0006] 3. Flame retardant VTM-0;

[0007] 4. Adhesive-to-adhesive peel strength at 35°C ≤ 0.2N / mm;

[0008] 5. Withstand voltage leakage current: at DC 2700V, the current is ≤1mA.

[0009] The technical problem to be solved by the present invention is to provide an adhesive and a preparation method thereof which can achieve the above five properties. Summary of the invention

[0010] The technical problem to be solved by the present invention is: to provide an adhesive capable of achieving the above five performances, wherein SKYBON saturated polyester ES-500 reacts with Wanhua toluene diisocyanate TD-80 to provide peeling strength; Toyobo saturated polyester GK780 reacts with Wanhua toluene diisocyanate TD-80 to provide peeling strength, and since the softening point of Toyobo saturated polyester GK780 is slightly higher than that of SKYBON saturated polyester ES-500, the peeling strength of adhesive to adhesive at 35°C can be reduced; aluminum hypophosphite OP935 reduces initial adhesion and adhesive to adhesive peeling strength, and also has a flame retardant effect; Wanhua toluene diisocyanate TD-80 cross-links with saturated polyester resin to improve the temperature resistance and adhesion performance of the system; BYK leveling agent BYK-302 makes the coating leveling good, the surface is uniform after coating, and the permeability of the system is improved, so that it can be well bonded to the 50um transparent PET coating substrate; xylene is used to dissolve the resin;

[0011] An adhesive for aerogel-covered hot-pressed film comprises the following components in percentage by mass: 31-37% of SKYBON saturated polyester ES-500; 6-8% of Toyobo saturated polyester GK780; 22% of aluminum hypophosphite OP935; 0.5-0.7% of Wanhua toluene diisocyanate TD-80; 0.08% of BYK leveling agent BYK-302; and the remainder of xylene.

[0012] Preferably, the composition comprises the following components in mass percentage: 33% of SKYBON saturated polyester ES-500; 7% of Toyobo saturated polyester GK780; 22% of aluminum hypophosphite OP935; 0.6% of Wanhua toluene diisocyanate TD-80; 0.08% of BYK leveling agent BYK-302; and the balance is xylene.

[0013] A method for preparing an adhesive for aerogel-covered hot-pressed film comprises the following steps:

[0014] S1: Use xylene to dissolve SKYBON saturated polyester ES-500 and Toyobo saturated polyester GK780 at a solid content of 30%;

[0015] S2: Slowly add aluminum hypophosphite OP935 to the mixed solution in S1 while stirring rapidly until it is evenly mixed;

[0016] S3: When it is cooled to ≤30°C, add Wanhua toluene diisocyanate TD-80, BYK leveling agent BYK-302 and the remaining xylene at the same time and stir for 15 minutes;

[0017] S4: Filter using 300 mesh filter cloth.

[0018] Compared with the prior art, the invention has the following beneficial effects: the invention is applied to the adhesive for aerogel-covered hot-pressed film, and can achieve the following five points: 1. Storage at 35°C for ≥3 months; 2. Peel strength after rapid hot pressing at low temperature of 110°C for 15S = 1.31N / mm; 3. Flame retardancy VTM-0; 4. Peel strength of adhesive to adhesive at 35°C = 0.06N / mm; 5. Withstand voltage leakage current, when DC is 2700V, the current is ≤1mA;

[0019] SKYBON saturated polyester ES-500 provides peel strength after reacting with Wanhua toluene diisocyanate TD-80; Toyobo saturated polyester GK780 provides peel strength after reacting with Wanhua toluene diisocyanate TD-80. In addition, since the softening point of Toyobo saturated polyester GK780 is slightly higher than that of SKYBON saturated polyester ES-500, it can reduce the peel strength of glue to glue at 35°C; aluminum hypophosphite OP935 reduces initial adhesion and glue to glue peel strength, and also has a flame retardant effect; Wanhua toluene diisocyanate TD-80 cross-links with saturated polyester resin to improve the temperature resistance and adhesion performance of the system; BYK leveling agent BYK-302 makes the coating leveling good, the surface is uniform after coating, and improves the permeability of the system, so that it has good adhesion with the 50um transparent PET coating substrate; xylene is used to dissolve the resin.

[0020] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In an embodiment of the present invention, an adhesive used for aerogel covering hot pressing film includes the following components in percentage by weight:

[0023] 31-37% SKYBON saturated polyester ES-500; it provides peel strength after reacting with Wanhua toluene diisocyanate TD-80;

[0024] 6-8% of Toyobo saturated polyester GK780; it provides peel strength after reacting with Wanhua toluene diisocyanate TD-80. In addition, since the softening point of Toyobo saturated polyester GK780 is slightly higher than that of SKYBON saturated polyester ES-500, it can reduce the peel strength of glue to glue at 35°C;

[0025] 22% aluminum hypophosphite OP935; it reduces initial adhesion, reduces adhesive-to-adhesive peel strength, and also has a flame retardant effect;

[0026] 0.5-0.7% Wanhua toluene diisocyanate TD-80; it cross-links with saturated polyester resin to improve the system's temperature resistance and adhesion properties;

[0027] 0.08% BYK leveling agent BYK-302; can make the coating leveling good, the surface uniform after coating, improve the permeability of the system, and make it adhere well to the 50um transparent PET coating substrate;

[0028] Xylene balance; its main function is to dissolve resin.

[0029] Further, the following components by mass percentage are included:

[0030] 33% SKYBON saturated polyester ES-500;

[0031] 7% Toyobo saturated polyester GK780;

[0032] 22% aluminum hypophosphite OP935;

[0033] 0.6% Wanhua toluene diisocyanate TD-80;

[0034] 0.08% BYK leveling agent BYK-302;

[0035] Xylene balance.

[0036] A method for preparing an adhesive for aerogel-covered hot-pressed film comprises the following steps:

[0037] S1: Use xylene to dissolve SKYBON saturated polyester ES-500 and Toyobo saturated polyester GK780 at a solid content of 30%;

[0038] S2: Slowly add aluminum hypophosphite OP935 to the mixed solution in S1 while stirring rapidly until it is evenly mixed;

[0039] S3: When it is cooled to ≤30°C, add Wanhua toluene diisocyanate TD-80, BYK leveling agent BYK-302 and the remaining xylene at the same time and stir for 15 minutes;

[0040] S4: Filter using 300 mesh filter cloth.

[0041] 1. Reasons for choosing SKYBON saturated polyester ES-500:

[0042] Effect of different saturated polyesters on peel strength (peel strength ≥ 0.8N / mm after rapid hot pressing at low temperature 110℃ and pressure 10KG / cm2 for 15S)

[0043] A. When the SKYBON saturated polyester ES-500 is replaced by other resins, its peel strength effect is as follows:

[0044] Saturated polyester type Peel strength N / mm SKBON’s ES-100 1.15 SKBON’s ES-120 1.17 SKBON's ES-300 1.21 SKBON’s ES-450 1.30 SKBON's ES-500 1.32 SKBON's ES-680 1.33 SKBON's ES-900 1.41 MARCOA C1110 1.39 MARCOA's G9530 1.25 MARCOA C7621 1.31

[0045] From this table, it can be concluded that the above resins all meet ≥0.8N / mm;

[0046] B. The effect of low-temperature pressing on the peel strength of adhesive to adhesive at 35°C (pressing for 15S, pressure 10KG / cm2, peel strength ≤0.2N / mm at 35°C).

[0047]

[0048]

[0049] The products that can meet both requirements A and B include ES-100, ES-120, ES-300, ES-450, and ES-500. The best one is ES-500, so SKYBON saturated polyester ES-500 is selected.

[0050] 2. Reasons for choosing Toyobo saturated polyester GK780:

[0051] Effect of different saturated polyesters on peel strength (peel strength ≥ 0.8N / mm after rapid hot pressing at low temperature 110℃ and pressure 10KG / cm2 for 15S)

[0052] A. When the Toyobo saturated polyester GK780 in the formula is replaced by other resins, its peel strength effect is as follows.

[0053] Saturated polyester type Peel strength N / mm Toyobo 220 0.48 Toyobo 270 0.65 Toyobo GK-360 0.71 Toyobo GK-880 0.66 Toyobo 560 1.41 Toyobo 670 1.44 Toyobo 600 1.15 Toyobo GK-780 1.31 MARCOA C7503 1.39 C1223 by MARCOA 1.24 SKBON ES-350 1.40

[0054] From this table, we can see that the resins that meet the conditions are Toyobo 560, 670, 600 and GK-780;

[0055] B. The influence of other resins replacing Toyobo saturated polyester GK780: The influence of low-temperature pressing on the peel strength of adhesive to adhesive at 35°C (pressing 15S, pressure 10KG / cm2, peel strength ≤0.2N / mm at 35°C).

[0056]

[0057]

[0058] From this table we can see that 220, 270, GK-360, GK880, 600, and GK-780 can meet the requirements.

[0059] Taking into account the comparative test results of A and B, Toyobo saturated polyester GK780 is preferred.

[0060] 3. Effect of the amount of Toyobo saturated polyester GK780 added on peel strength (low temperature 110℃, pressure 10KG / cm 2After rapid hot pressing for 15S, the peel strength should be ≥0.8N / mm)

[0061] GK-780 addition amount% Peel strength N / mm 2 1.29 3 1.31 4 1.30 5 1.31 6 1.30 7 1.31 8 1.30 9 1.28 10 1.27 11 1.26

[0062] From this table, it can be seen that the addition of Toyobo saturated polyester GK780 has a small effect on the overall peeling strength after lamination.

[0063] Effect of the addition amount of Toyobo saturated polyester GK780 on peel strength (pressing 15S, pressure 10KG / cm 2 , peel strength ≤0.2N / mm at 35℃)

[0064]

[0065]

[0066] From this table, it can be seen that the addition amount of Toyobo saturated polyester GK780 from 3 to 12% can meet the peel strength requirement of ≤0.2N / mm.

[0067] Considering the effects at 110°C and 35°C, 6-8% is preferred.

[0068] 4. Effect of SKYBON saturated polyester ES-500 addition on peel strength (low temperature 110℃, pressure 10KG / cm 2 After rapid hot pressing for 15S, the peel strength should be ≥0.8N / mm)

[0069] ES-500 addition amount% Peel strength N / mm 25 1.12 27 1.18 29 1.21 31 1.25 33 1.31 35 1.32 37 1.32 39 1.32 41 1.32 43 1.32 45 1.32

[0070] From this table, we can see that when the addition amount of SKYBON saturated polyester ES-500 increases gradually from 25% to 45%, its peel strength approaches the maximum value at 33%, and further increase has almost no change on the peel strength.

[0071] Effect of SKYBON saturated polyester ES-500 addition on flame retardancy (pressing 15S, pressure 10KG / cm2, peel strength ≤0.2N / mm at 35℃)

[0072] ES-500 addition amount% Flame retardant effect 25 VTM-0 27 VTM-0 29 VTM-0 31 VTM-0 33 VTM-0 35 VTM-0 37 VTM-0 39 VTM-1 41 VTM-1 43 VTM-1 45 VTM-2

[0073] As the addition amount of SKYBON saturated polyester ES-500 increases, the flame retardant powder will be relatively reduced, resulting in reduced flame retardancy. When the addition amount of SKYBON saturated polyester ES-500 is ≤37%, the VTM-0 effect can be achieved.

[0074] Considering the data in the above two tables, the best range of SKYBON saturated polyester ES-500 is 31-37%.

[0075] 5. Effect of the addition amount of Wanhua toluene diisocyanate TD-80 on peel strength (low temperature 110℃, pressure 10KG / cm 2 After rapid hot pressing for 15S, the peel strength should be ≥0.8N / mm)

[0076] TD-80 addition amount% Peel strength N / mm 0.2 0.94 0.3 1.17 0.4 1.24 0.5 1.28 0.6 1.31 0.7 1.30 0.8 1.30 0.9 1.27 1.0 1.25

[0077] From this table, we can see that when the addition amount of Wanhua toluene diisocyanate TD-80 is 0.6-0.8%, the peel strength reaches the maximum value;

[0078] Effect of the addition amount of Wanhua toluene diisocyanate TD-80 on peel strength (low temperature 110℃, pressure 10KG / cm 2 After rapid hot pressing for 15S, the peel strength should be ≥0.8N / mm)

[0079] TD-80 addition amount% Peel strength N / mm 0.2 0.18 0.3 0.12 0.4 0.08 0.5 0.06 0.6 0.06 0.7 0.06 0.8 0.06 0.9 0.06 1.0 0.06

[0080] From the above two tables, it can be seen that Wanhua toluene diisocyanate TD-80 can meet the requirements when the addition amount is in the range of 0.2-1.0%. In order to achieve better results, considering the effects at 110℃ and 35℃, Wanhua toluene diisocyanate TD-80 is preferably 0.5-0.7%.

[0081] 6. This application can achieve the following under bare conditions:

[0082] 1. Storage at 35℃ for ≥3 months; 2. Low temperature 110℃, 15S rapid hot pressing after peel strength = 1.31N / mm; 3. Flame retardancy VTM-0; 4. Adhesive to adhesive 35℃ peel strength = 0.06N / mm; 5. Withstand voltage leakage current, DC 2700V, current ≤1mA;

[0083] During high temperature lamination, the influence of lamination temperature on peel strength:

[0084]

[0085]

[0086] From this table, it can be concluded that the pressing temperature has a great influence on its peel strength. The higher the pressing temperature, the higher the peel strength. When the temperature is ≥85℃, the peel strength can achieve the desired effect.

[0087] Effect of Lamination Time on Peel Strength:

[0088] <![CDATA[Laminating time S (laminating temperature is 115 °C, pressure is 10 KG / cm 2 )]]> Peel strength N / mm 10 1.14 11 1.19 12 1.24 13 1.28 14 1.32 15 1.37 16 1.40 17 1.40 18 1.42 19 1.44 20 1.45 21 1.46

[0089] From this table, it can be concluded that when the pressing time is within 10 to 21 seconds, the peel strength can meet the requirement of ≥0.8N / mm.

[0090] Effect of adhesive coating thickness on peel strength (required 27~33μm)

[0091] Glue coating thickness (dry glue) μm Peel strength N / mm 27 1.30 28 1.31 29 1.33 30 1.35 31 1.35 32 1.36 33 1.37

[0092] From this table, it can be concluded that when the coating thickness ranges from 27 to 33μm, the peel strength can meet the requirement of ≥0.8N / mm.

[0093] Effect of adhesive coating thickness on flame retardancy (tested after adhesive drying)

[0094] Glue coating thickness (dry glue) μm Flame retardancy grade 27 VTM-0 28 VTM-0 29 VTM-0 30 VTM-0 31 VTM-0 32 VTM-0 33 VTM-0

[0095] From this table, it can be concluded that when the coating thickness is between 27 and 33 μm, the VTM-0 flame retardant grade can be achieved.

[0096] Effect of the addition amount of aluminum hypophosphite OP935 on flame retardancy:

[0097] OP935 addition% (coating thickness is 27μm) Flame retardancy grade 14 VTM-2 16 VTM-2 18 VTM-1 20 VTM-1 22 VTM-0 24 VTM-0 26 VTM-0

[0098] From this table, it can be concluded that when the coating thickness is between 22% and 26%, the VTM-0 flame retardant grade can be achieved.

[0099] The influence of low-temperature pressing on the peel strength of adhesive to adhesive at 35°C (pressing 15S, pressure 10KG / cm2, peel strength ≤0.2N / mm at 35°C).

[0100]

[0101]

[0102] From this table, it can be concluded that within the test temperature range, the higher the temperature, the higher the peel strength, but all meet the requirement of peel strength ≤ 0.2N / mm at 35°C.

[0103] The comprehensive test results of this formula under the conditions of use: 110℃, 15S, pressure 10KG / cm2 are as follows:

[0104]

[0105] Low temperature 35℃, 15S, pressure 10KG / cm 2 Press fit test results

[0106]

[0107] After 4 months of storage at room temperature: 110℃, 15S, pressure 10KG / cm 2 The comprehensive test results are shown in the table below.

[0108]

[0109]

[0110] After 4 months of storage at room temperature: low temperature 35℃, 15S, pressure 10KG / cm 2 Press fit test results

[0111]

[0112] In summary, this formula can meet the five requirements of the market:

[0113] 1. Can be stored at 35℃ for at least 3 months under exposed conditions; 2. Low temperature 110℃, peel strength after 15S rapid hot pressing ≥0.8N / mm; 3. Flame retardancy VTM-0; 4. Adhesive to adhesive peel strength at 35℃ ≤0.2N / mm; 5. Withstand voltage leakage current, at DC 2700V, the current is ≤1mA.

[0114] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. An adhesive for aerogel-covered hot-pressed film, characterized in that: Includes the following mass percentage components: 31-37% SKYBON saturated polyester ES-500; 6-8% Toyobo saturated polyester GK780; 22% aluminum hypophosphite OP935; 0.5-0.7% Wanhua toluene diisocyanate TD-80; 0.08% BYK leveling agent BYK-302; Xylene balance.

2. The adhesive for aerogel-covered hot-pressed film according to claim 1, characterized in that: Includes the following mass percentage components: 33% SKYBON saturated polyester ES-500; 7% Toyobo saturated polyester GK780; 22% aluminum hypophosphite OP935; 0.6% Wanhua toluene diisocyanate TD-80; 0.08% BYK leveling agent BYK-302; Xylene balance.

3. A preparation method for preparing the adhesive for aerogel-covered hot-pressed film as claimed in any one of claims 1 to 2, comprising the following steps: S1: Use xylene to dissolve SKYBON saturated polyester ES-500 and Toyobo saturated polyester GK780 at a solid content of 30%; S2: Slowly add aluminum hypophosphite OP935 to the mixed solution in S1 while stirring rapidly until it is evenly mixed; S3: When it is cooled to ≤30°C, add Wanhua toluene diisocyanate TD-80, BYK leveling agent BYK-302 and the remaining xylene at the same time and stir for 15 minutes; S4: Filter using 300 mesh filter cloth.