Organic long-afterglow thin film material based on blue phosphorescence as well as preparation method and application of organic long-afterglow thin film material

By combining polymethyl methacrylate, triphenylphosphine and 4,4'-azadiyldibenzoic acid, an organic long afterglow film material with high-efficiency blue afterglow performance was prepared, which solved the difficulty in the prior art The problem of efficient blue light emission and large-area coating has been realized, and applications in flexible display, wearable devices and anti-counterfeiting fields are realized.

CN118909618APending Publication Date: 2024-11-08HEBEI PETROLEUM VOCATIONAL & TECH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410969253.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to develop high-efficiency blue-ray emission and large-area coating organic long afterglow film materials, limiting their commercial applications in the fields of flexible displays, wearable devices and anti-counterfeiting.

Method used

Polymethyl methacrylate, triphenylphosphine and 4,4'-azabidylbenzoic acid are used as main body and guest materials, and a thin film material with blue afterglow properties is prepared by heating stirring and cooling processes. The mass ratio is 100:30:1 and the excitation wavelength is 360~380nm, achieving high-efficiency blue afterglow emission.

Benefits of technology

The prepared film material has an afterglow time of up to 6 seconds and a blue afterglow color, which is suitable for large-area coating, suitable for flexible display, wearable devices and anti-counterfeiting fields, is cheap and easy to obtain, and is suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909618A_ABST
    Figure CN118909618A_ABST
Patent Text Reader

Abstract

The invention relates to the field of organic afterglow thin film materials, in particular to an organic long-afterglow thin film material based on blue phosphorescence and a preparation method and application of the organic long-afterglow thin film material. According to the organic long-afterglow thin film material based on blue phosphorescence provided by the invention, polymethyl methacrylate is used as a first component of a main body material, an electron-rich material triphenylphosphine which is low in price and easy to obtain is introduced as a second component of the main body material, and 4, 4 '-diphenyl-1, 2, 3-triazole is further introduced, so that the organic long-afterglow thin film material is prepared. 4, 4 '-aza-diyl dibenzoic acid is used as a guest material, and a novel blue long-afterglow luminescent material is constructed. The material has blue long-afterglow luminescence in a room-temperature atmospheric environment, the afterglow time exceeds 6s, and large-area coating preparation can be carried out. Therefore, a simple strategy can be provided for developing the ultra-wide-range, tunable-service-life, efficient and lasting dark blue room temperature phosphorescent material, and a theoretical basis and a material basis can also be provided for practical applications such as data encryption, counterfeiting prevention, flexible display devices and wearable equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic afterglow film materials, and in particular to an organic long afterglow film material based on blue phosphorescence and a preparation method and application thereof. Background Art

[0002] With the rapid growth of application demand, the development space of my country's organic light-emitting materials industry continues to expand. Blue phosphorescent materials refer to organic compounds that can emit blue phosphorescence, and belong to the second generation of organic light-emitting materials. Compared with other organic light-emitting materials, blue phosphorescent materials have the advantages of long service life, high color purity, high luminous efficiency and energy conversion efficiency, and can be used to produce display devices such as OLED panels. The latest market research on the blue phosphorescent materials industry shows that the display panel field is currently the largest demand side for blue phosphorescent materials. In the future, with the accelerated development of organic light-emitting materials and OLED panel industries, the market share and application demand of blue phosphorescent materials will become increasingly strong.

[0003] At present, many studies have reported a variety of high-efficiency room-temperature phosphorescent materials, but most of the materials are green or red, and there are relatively few blue materials, especially the research on room-temperature phosphorescent blue materials with wide range and adjustable lifetime. As one of the three primary colors, blue is crucial for the production of white light-emitting devices. However, since good phosphorescent luminophores usually have large conjugated structures and phosphorescence has a large Stokes shift relative to fluorescence, its emission wavelength is concentrated in the range of 500-600nm. Therefore, it is challenging to achieve deep blue room-temperature phosphorescent materials with adjustable lifetime, high efficiency and long-lasting.

[0004] In addition, due to the characteristics of organic compounds themselves, singlet and triplet intersystem crossing is transition-forbidden and is sensitive to temperature and air, so it is difficult to achieve long-life, high-efficiency organic long afterglow emission. At present, the solution to this problem is to increase the organic afterglow time, luminescence brightness and afterglow color by establishing a rigid environment, crystallization, host-guest doping, H-aggregates, etc. However, the afterglow materials prepared by the above methods are generally fragile and difficult to coat over a large area and emit light uniformly, which seriously limits the commercial application of such materials in flexible displays, wearable and portable electronic devices, and anti-counterfeiting.

[0005] Therefore, how to develop thin film materials that can emit blue light with high efficiency and can be coated on a large area so as to be effectively applied in flexible display technology, wearable devices, organic optoelectronic information and high-end anti-counterfeiting fields is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of this, the first aspect of the present invention is to provide an organic long afterglow thin film material based on blue phosphorescence, the raw materials for its preparation are cheap and easily available, the afterglow life is long and the afterglow color is blue, it can be coated on a large area and emit light uniformly, and is suitable for applications in flexible display technology, wearable devices, organic optoelectronic information and high-end anti-counterfeiting.

[0007] The second aspect of the present invention is to provide a method for preparing an organic long afterglow thin film material based on blue phosphorescence. The preparation method is simple, the material is cheap and easily available, the conditions are mild and do not require harsh conditions such as high temperature and high pressure. It can prepare a thin film material that emits blue light with high efficiency and can be coated on a large area.

[0008] The third aspect of the present invention is to provide the application of the above-mentioned organic long afterglow thin film material based on blue phosphorescence.

[0009] The first aspect of the present invention is implemented by the following technical solution:

[0010] The organic long afterglow thin film material based on blue phosphorescence is prepared by heating and cooling a main material and a guest material; the main material is polymethyl methacrylate and triphenylphosphine; the guest material is 4,4'-azadiyldibenzoic acid;

[0011] The mass ratio of polymethyl methacrylate, triphenylphosphine and 4,4'-azadiyldibenzoic acid is (80-120):(20-40):1; and the relative molecular mass of the polymethyl methacrylate is 10000-15000.

[0012] In consideration of improving the afterglow time and regulating the afterglow color, the mass ratio of polymethyl methacrylate, triphenylphosphine and 4,4'-azadiyldibenzoic acid is 100:30:1.

[0013] Furthermore, the relative molecular mass of the polymethyl methacrylate is 13000.

[0014] Furthermore, the excitation wavelength of the organic long afterglow thin film material based on blue phosphorescence is 360-380 nm, more preferably 365 nm.

[0015] The second aspect of the present invention is implemented by the following technical solution:

[0016] The method for preparing an organic long afterglow thin film material based on blue phosphorescence comprises the following steps:

[0017] S1, mixing the main material and the guest material uniformly to obtain a solid powder;

[0018] S2. The solid powder is heated and stirred, and then cooled to form a film, so as to obtain the organic long afterglow thin film material based on blue phosphorescence.

[0019] Furthermore, the process conditions of heating and stirring are: heating temperature 140-180° C., stirring speed 200-1000 rpm.

[0020] Furthermore, the heating and stirring time is 2 to 12 minutes.

[0021] Furthermore, the cooling film forming is performed by standing and cooling at a temperature of 15 to 30°C.

[0022] The third aspect of the present invention is implemented by the following technical solution:

[0023] The above-mentioned application of the organic long afterglow thin film material based on blue phosphorescence is used as a thin film material in data encryption systems, anti-counterfeiting elements, flexible display devices or wearable devices.

[0024] The main beneficial effects of the present invention are:

[0025] (i) The organic long afterglow film material based on blue phosphorescence provided by the present invention uses polymethyl methacrylate as the first component of the main material, and introduces triphenylphosphine, a cheap and easily available electron-rich material, as the second component of the main material, and further introduces 4,4'-azadiyldibenzoic acid as the guest material to construct a new type of blue long afterglow luminescent material. The afterglow time of this material exceeds 6s and the afterglow color is blue, and it has good blue afterglow luminescence performance. Therefore, the present invention only constructs a rigid environment through a polymer substrate and regulates the energy transfer between the host and the guest, thereby achieving the successful preparation of a blue afterglow luminescent phosphorescent material with relatively large technical barriers, demonstrating its application potential in the fields of information encryption and anti-counterfeiting.

[0026] (ii) On the one hand, when determining the material, the present invention selects polymethyl methacrylate as the matrix for film construction. The polymer film can not only provide a rigid environment to suppress the non-radiative transition of the guest molecules, but also Resonance energy transfer (FRET) enables the host molecule and the guest molecule to work synergistically in the photophysical process, thereby enhancing the afterglow time of the thin film material. The present invention further selects triphenylphosphine, which is the key to the melting of polymethyl methacrylate at a certain temperature. At the same time, triphenylphosphine can not only form energy transfer with the guest, but also cooperate with the polymer to form a dense rigid environment; finally, the present invention selects 4,4'-azadiyldibenzoic acid as the guest material, which can work synergistically with the host polymer and triphenylphosphine to form a blue afterglow luminescence effect. The improvement of the long afterglow performance of blue is very beneficial to promote the application of materials in fields such as OLED panels based on blue phosphorescence.

[0027] On the other hand, when preparing materials, the present invention starts from the perspective of increasing the afterglow time of organic long afterglow thin film materials and regulating the color, and dopes a small amount of electronic guest materials into the main material by heating and melting, cooling and solidifying, thereby successfully constructing a new type of thin film material, which has a simple preparation method, cheap and easy-to-obtain materials, mild conditions, and does not require harsh conditions such as high temperature and high pressure, and can prepare a thin film material that emits blue light efficiently and can be coated on a large area. The successful preparation of thin film materials with good film morphology and large-area coating preparation is very conducive to the commercial application of such materials in flexible displays, wearable and portable electronic devices, and anti-counterfeiting.

[0028] (iii) The host and guest materials of current afterglow materials are generally complex and expensive, while the organic long afterglow thin film material based on blue phosphorescence used in the present invention is cheap, easy to obtain, and has a simple structure, which provides more possibilities for its actual commercial application. In addition, the material provided by the present invention can be excited by ultraviolet light, has the characteristics of environmental stability, and can form a regular transparent film, with an afterglow performance of up to 6s, which is better than conventional afterglow materials.

[0029] Therefore, the present invention is aimed at the research on organic long afterglow thin film materials based on blue phosphorescence. The polymer substrate provides a rigid environment to suppress non-radiative transitions and disperse the luminophores to avoid aggregation-induced luminescence red shift. This not only provides new ideas for the design and synthesis of new blue thin film long afterglow materials, but also provides a simple strategy for the development of ultra-wide range tunable life and high-efficiency and long-lasting deep blue room temperature phosphorescent materials. It can provide a theoretical basis and material foundation for practical applications such as data encryption, anti-counterfeiting, flexible display devices, and wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The optical images of the afterglow display of the organic long afterglow thin film material based on blue phosphorescence in Example 1 of the present invention before (a) and after (bh) irradiation with 365nm ultraviolet light;

[0031] Figure 2 This is a graph showing the afterglow performance attenuation curve of the organic long afterglow thin film material based on blue phosphorescence according to Example 1 of the present invention;

[0032] Figure 3 The optical images of the afterglow display of the organic thin film material of Comparative Example 1 before (a) and after (bd) irradiation with 365nm ultraviolet light;

[0033] Figure 4 The optical images of the afterglow display of the organic thin film material of Comparative Example 3 before (a) and after (bf) irradiation with 365nm ultraviolet light;

[0034] Figure 5This is a graph showing the afterglow performance attenuation curve of the organic thin film material of Comparative Example 3. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below in conjunction with specific embodiments and drawings, but the protection scope of the present invention is not limited thereto. The experimental methods used in the following embodiments are conventional methods unless otherwise specified; the raw materials used are commonly used in the art, available to the public or commercially available unless otherwise specified; the terms and abbreviations involved have conventional meanings in the art.

[0036] In the following examples, the host material and the guest material used are all purchased from manufacturers. The relative molecular mass of the polymethyl methacrylate used in the following examples or comparative examples is 13,000.

[0037] Example 1

[0038] The organic long afterglow film material based on blue phosphorescence provided in this embodiment is prepared by heating and cooling a host material and a guest material; the host material is polymethyl methacrylate and triphenylphosphine The guest material is 4,4'-azadiyldibenzoic acid

[0039] Among them, the host material forms a regular transparent film, and the guest material is freely dispersed in the film of the host material.

[0040] The method for preparing the above-mentioned organic long afterglow thin film material based on blue phosphorescence comprises the following steps:

[0041] (1) According to the mass ratio of the host material (polymethyl methacrylate: triphenylphosphine) to the guest material (4,4'-azadiyldibenzoic acid) of 100:30:1; accurately weigh 0.0010 g of the guest material (4,4'-azadiyldibenzoic acid), 0.1000 g of the host material (polymethyl methacrylate), and 0.030 g of the host material (triphenylphosphine) and mix them to obtain a solid powder;

[0042] (2) The solid powder is placed in an oil bath and heated to 160°C for heating and stirring at a stirring speed of 600 rpm. Stir for 5 minutes until it is completely dissolved, and then keep it in the oil bath for 1 minute. Finally, the material is taken out and placed in an atmospheric environment at room temperature of 20 to 25°C, and slowly cooled to form a thin film, thereby obtaining the blue phosphorescent organic long afterglow thin film material of Example 1.

[0043] Comparative Example 1

[0044] This comparative example provides an organic thin film material, and its preparation method is as follows:

[0045] (1) According to the mass ratio of the host material (triphenylphosphine) to the guest material (4,4'-azadiyldibenzoic acid) of 30:1; accurately weigh 0.0010 g of the guest material (4,4'-azadiyldibenzoic acid) and 0.030 g of the host material (triphenylphosphine) and mix them to obtain a solid powder;

[0046] (2) The solid powder is placed in an oil bath and heated to 160°C for heating and stirring at a stirring speed of 600 rpm for 5 minutes until it is completely dissolved, and then kept in the oil bath for 1 minute. Finally, the material is taken out and placed in an atmospheric environment at room temperature of 20 to 25°C, and slowly cooled to form a thin film, thereby obtaining the organic thin film material of Comparative Example 1.

[0047] Comparative Example 2

[0048] This comparative example provides an organic thin film material, and its preparation method is as follows:

[0049] (1) According to the mass ratio of the host material (polymethyl methacrylate) to the guest material (4,4'-azadiyldibenzoic acid) of 100:1; accurately weigh 0.0010 g of the guest material (4,4'-azadiyldibenzoic acid) and 0.1000 g of the host material (polymethyl methacrylate) and mix them to obtain a solid powder;

[0050] (2) The solid powder is placed in an oil bath and heated to 160°C for heating and stirring at a stirring speed of 600 rpm for 5 minutes until it is completely dissolved, and then kept in the oil bath for 1 minute. Finally, the material is taken out and placed in an atmospheric environment at room temperature of 20 to 25°C, and slowly cooled to form a thin film, thereby obtaining the organic thin film material of Comparative Example 2.

[0051] Comparative Example 3

[0052] This comparative example provides an organic thin film material, and its preparation method is as follows:

[0053] (1) According to the mass ratio of the host material (polymethyl methacrylate: triphenylphosphine) to the guest material (4-diphenylaminobenzaldehyde) of 100:30:1; accurately weigh 0.0010 g of the guest material (4-diphenylaminobenzaldehyde), 0.1000 g of the host material (polymethyl methacrylate), and 0.030 g of the host material (triphenylphosphine) and mix them to obtain a solid powder;

[0054] The structural formula of the guest material 4-diphenylaminobenzaldehyde is:

[0055]

[0056] (2) The solid powder is placed in an oil bath and heated to 160°C for heating and stirring at a stirring speed of 600 rpm for 5 minutes until it is completely dissolved, and then kept in the oil bath for 1 minute. Finally, the material is taken out and placed in an atmospheric environment at room temperature of 20 to 25°C, and slowly cooled to form a thin film, thereby obtaining the organic thin film material of Comparative Example 3.

[0057] Comparative Example 4

[0058] This comparative example provides an organic thin film material, and its preparation method is as follows:

[0059] (1) According to the mass ratio of the host material (polymethyl methacrylate: triphenylphosphine) to the guest material (pentacene) of 100:30:1, 0.0010 g of the guest material (pentacene), 0.1000 g of the host material (polymethyl methacrylate) and 0.030 g of the host material (triphenylphosphine) were accurately weighed and mixed to obtain a solid powder;

[0060] The structural formula of the guest material pentacene is:

[0061]

[0062] (2) The solid powder is placed in an oil bath and heated to 160°C for heating and stirring at a stirring speed of 600 rpm for 5 minutes until it is completely dissolved, and then kept in the oil bath for 1 minute. Finally, the material is taken out and placed in an atmospheric environment at room temperature of 20 to 25°C, and slowly cooled to form a thin film, thereby obtaining the organic thin film material of Comparative Example 4.

[0063] Test Example 1: Performance test of film material of Example 1

[0064] Under room temperature and atmospheric environment, the organic long afterglow film material of Example 1 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the afterglow brightness change of the film material after the light source was removed was recorded. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the 365nm ultraviolet lamp excites the film material of Example 1 ( Figure 1 a), turn off the excitation light source. After the light source is removed, the film material emits a blue afterglow ( Figure 1 b) In the first 5 seconds, Figure 1 b~1f represent the changes in the afterglow performance of the material after the light source is removed for 1s, 2s, 3s, 4s, and 5s, respectively. In the 1~5s after the light source is removed, the afterglow brightness of the material is strong, and from the 5.5s ( Figure 1 g) and then the afterglow gradually weakened, and at 6.0s ( Figure 1 h) The afterglow is not obvious. It can be seen that the blue afterglow time of the thin film material of Example 1 is as high as 6.0s, which has excellent blue afterglow performance.

[0065] The afterglow performance attenuation of the organic long afterglow film material of Example 1 was further tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that -2s to 0s is the performance of the material of Example 1 under the irradiation of 365nm ultraviolet lamp, which exhibits photoluminescence characteristics; 0s to 8s is the performance of the material of Example 1 after the ultraviolet lamp is removed, which exhibits long blue afterglow light, and the afterglow time is about 6.3s, which is similar to the afterglow time observed by the naked eye.

[0066] Test Example 2: Performance Test of Thin Film Materials of Comparative Examples 1 to 4

[0067] (1) Test results of comparative example 1

[0068] Under room temperature and atmospheric environment, the organic thin film material of Comparative Example 1 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the afterglow brightness change of the material after the light source was removed was recorded. Figure 3 As shown. Figure 3 It can be seen that the 365nm ultraviolet lamp excites the film material of Comparative Example 1 ( Figure 3 a), turn off the excitation light source. After the light source is removed, the film material emits a turquoise afterglow ( Figure 3 b). Figure 3 b~3c represent the results of removing the light source after 1s, 1.5s, and 2s respectively. In the first 1.5s, the afterglow brightness of the material is strong. Figure 3 c) and then the afterglow gradually weakens. Figure 3 d) The afterglow is not obvious. It can be seen that the afterglow time of the thin film material of Comparative Example 1 is only 2s, and the afterglow color is green, which means that when the guest material 4,4'-azadiyldibenzoic acid and the host material triphenylphosphine react, green afterglow light is emitted, and the afterglow time is short.

[0069] (2) Comparative Example 2 Test Results

[0070] Under room temperature and atmospheric environment, after exciting the organic thin film material of comparative example 2 with a 365nm ultraviolet lamp, the excitation light source was turned off, and the afterglow brightness change of the thin film material after the light source was removed was recorded. The test results show that the thin film material does not have any color of light after the light source is removed, indicating that only using polymethyl methacrylate as the host material and the guest material 4,4'-azadiyldibenzoic acid as the role, can not stimulate the afterglow performance.

[0071] (3) Test results of comparative example 3

[0072] Under room temperature and atmospheric environment, the organic thin film material of comparative example 3 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the afterglow brightness change of the thin film material after the light source was removed was recorded. Figure 4 As shown. Figure 4 It can be seen that the 365nm ultraviolet lamp excites the film material of Comparative Example 3 ( Figure 4 a), turn off the excitation light source. After the light source is removed, the film material emits a green afterglow ( Figure 4 b) In the first 3 seconds, Figure 4 b~4d represent the results of removing the light source in the first second, second second, and third second, respectively. During this time, the afterglow brightness of the compound is relatively strong. From the 3rd second (such as Figure 4 e) and then the afterglow gradually weakened, and the 4th second ( Figure 4 f) The afterglow is not obvious. It can be seen that the afterglow time of the film material of Comparative Example 3 is only 4s, and the afterglow color is green. This shows that when the structure of the guest material is changed and a guest material with other structures such as 4-diphenylaminobenzaldehyde is used to react with the host material (triphenylphosphine and polymethyl methacrylate), although the afterglow time is moderate, the afterglow emitted is green, and it is difficult to achieve a blue afterglow.

[0073] The afterglow performance attenuation of the organic thin film material of Comparative Example 3 was further tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 5 shown. Figure 5 In the figure, -2s to 0s are the results of the organic thin film material of Comparative Example 3 under 365nm ultraviolet light, which exhibits photoluminescence characteristics; 0s to 8s are the results of the organic thin film material of Comparative Example 3 after the ultraviolet light is removed, which exhibits green long afterglow light, and the afterglow time is about 4.1s, which is similar to the afterglow time observed by the naked eye.

[0074] (4) Comparative Example 4 Test Results

[0075] Under room temperature and atmospheric environment, after exciting the organic thin film material of comparative example 4 with a 365nm ultraviolet lamp, the excitation light source is turned off, and the change in the afterglow brightness of the thin film material after the light source is removed is recorded. The test results show that the afterglow time of the thin film material of comparative example 4 is only 1s, and the afterglow color is green. This shows that when the structure of the guest material is changed and other guest materials such as pentacene are used to react with the host material (triphenylphosphine and polymethyl methacrylate), green afterglow performance is emitted, and it is difficult to achieve blue afterglow, and the green afterglow performance of the material is relatively short.

[0076] In summary, the present invention focuses on the research of organic long afterglow thin film materials based on blue phosphorescence, which not only provides new ideas for the design and synthesis of new blue long afterglow materials, but also provides theoretical basis and material foundation for practical applications such as data encryption systems, anti-counterfeiting elements, flexible display devices, and wearable devices.

Claims

1. An organic long afterglow thin film material based on blue phosphorescence, characterized in that: The organic long afterglow thin film material based on blue phosphorescence is prepared by heating and cooling a main material and a guest material; the main material is polymethyl methacrylate and triphenylphosphine; the guest material is 4,4'-azadiyldibenzoic acid; The mass ratio of polymethyl methacrylate, triphenylphosphine and 4,4'-azadiyldibenzoic acid is (80-120):(20-40):1; and the relative molecular mass of the polymethyl methacrylate is 10000-15000.

2. The organic long afterglow thin film material based on blue phosphorescence according to claim 1, characterized in that: The mass ratio of polymethyl methacrylate, triphenylphosphine and 4,4'-azadiyldibenzoic acid is 100:30:

1.

3. The organic long afterglow thin film material based on blue phosphorescence according to claim 1, characterized in that: The relative molecular mass of the polymethyl methacrylate is 13000.

4. The organic long afterglow thin film material based on blue phosphorescence according to claim 1, characterized in that: The excitation wavelength of the organic long afterglow thin film material based on blue phosphorescence is 360-380 nm.

5. A method for preparing an organic long afterglow thin film material based on blue phosphorescence according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, mixing the main material and the guest material uniformly to obtain a solid powder; S2. The solid powder is heated and stirred, and then cooled to form a film, so as to obtain the organic long afterglow thin film material based on blue phosphorescence.

6. The method for preparing an organic long afterglow thin film material based on blue phosphorescence according to claim 5, characterized in that: The process conditions of heating and stirring are: heating temperature 140-180° C., stirring speed 200-1000 rpm.

7. The method for preparing an organic long afterglow thin film material based on blue phosphorescence according to claim 5, characterized in that: The heating and stirring time is 2 to 12 minutes.

8. The method for preparing an organic long afterglow thin film material based on blue phosphorescence according to claim 5, characterized in that: The cooling film forming is performed by cooling at 15 to 30°C.

9. An application of an organic long afterglow thin film material based on blue phosphorescence as claimed in any one of claims 1 to 4, characterized in that: Application as thin film material in data encryption systems, anti-counterfeiting elements, flexible display devices or wearable devices.

Citation Information

Cited By

  • Organic long-afterglow material capable of stably emitting light in severe environment and preparation method of organic long-afterglow material

    CN121159917A