Application of copper-gold nano-cluster / carbon quantum dot ratiometric fluorescent probe in detection of aflatoxin
Through the copper-gold nanocluster/carbon quantum dot ratio fluorescence probe, the problem of long detection time, high cost and large signal error in the existing aflatoxin detection method is solved, and the problem of long detection time, high cost and large signal error is achieved. Fast and accurate aflatoxin detection, with high sensitivity and anti-interference.
Patent Information
- Application Number
- CN202410922880.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing aflatoxin detection methods have cumbersome pre-processing, long detection time, expensive cost and large signal background errors, which cannot meet the needs of fast on-site detection.
Using copper-gold nanoclusters/carbon quantum dot ratio fluorescent probe, the copper-gold nanoclusters and silica-coated carbon quantum dots are mixed, and the Hg2+ ion-mediated fluorescence quenching effect is achieved. Accurate and fast detection.
Fast and accurate detection of aflatoxin is achieved, background error is reduced, high sensitivity and anti-interference, and no expensive chromatograph is required. The minimum detection limit for detection is 0.56ng/mL, and the linear range is 0. ~55ng/mL, sensitivity is 33.15mL/ng, and good selectivity and anti-interference.
Smart Images

Figure CN118909622A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ratio fluorescent probes, and in particular to application of a copper-gold nanocluster / carbon quantum dot ratio fluorescent probe in detecting aflatoxin. Background Art
[0002] Aflatoxins (AFs) are a class of secondary metabolites of heterocyclic aromatic hydrocarbons, mainly produced by Aspergillus flavus and Aspergillus parasiticus under hot and humid conditions. The World Health Organization has classified them as Class I carcinogens. Aflatoxins have derivatives such as B1, B2, G1, G2, M1, M2, GM, P1, and Q1. Among them, aflatoxin B1 (AFB1) is the strongest known natural carcinogen with the highest toxicity. AFB1 is highly carcinogenic, mutagenic, and teratogenic, and can induce primary liver cancer, gastric cancer, lung cancer, etc. It is also the main risk factor in the multifactorial etiology of human hepatocellular carcinoma (HCC).
[0003] At present, the main methods used for aflatoxin detection include thin layer chromatography (TLC), high performance liquid chromatography (HPLC), high performance liquid chromatography-mass spectrometry (HPLC-MS), enzyme-linked immunosorbent assay (ELISA), etc. These methods have defects such as cumbersome sample pretreatment, lengthy detection time, expensive testing costs and demanding testing equipment, and cannot meet the needs of rapid on-site detection of AFs. Fluorescence detection has attracted the attention of researchers due to its advantages such as strong specificity, high sensitivity and simple operation, but the current fluorescence detection method relies on the output change of a single signal, and its background error and environmental error cannot be eliminated. Summary of the invention
[0004] In order to solve the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide an application of a copper-gold nanocluster / carbon quantum dot ratio fluorescent probe in the detection of aflatoxin, so as to achieve accurate and rapid detection of aflatoxin.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: provide a copper-gold nanocluster / carbon quantum dot ratio fluorescent probe for use in detecting aflatoxin, and the copper-gold nanocluster / carbon quantum dot ratio fluorescent probe is prepared by the following method: copper-gold nanoclusters and silica-coated carbon quantum dots are mixed to obtain the probe.
[0006] Furthermore, the volume ratio of the copper-gold nanoclusters and the silicon dioxide-coated carbon quantum dots is 1:3-6.
[0007] Furthermore, the copper-gold nanoclusters are prepared by the following method: using chloroauric acid and copper salt as raw materials and glutathione as a ligand, the copper-gold nanoclusters are prepared by a chemical reduction method.
[0008] Furthermore, the copper-gold nanoclusters are prepared by the following method: CuCl2·2H2O solution, HAuCl4·4H2O solution and glutathione solution are uniformly mixed and reacted for 20-40 minutes, and then the reaction system is adjusted to acidic and the reaction is continued for 60-90 minutes to obtain the copper-gold nanoclusters.
[0009] Furthermore, the molar ratio of CuCl2·2H2O, HAuCl4·4H2O and glutathione is 45-55:1:85-95.
[0010] Furthermore, the reaction system is adjusted to be acidic by adjusting the pH of the reaction system to 3-5.
[0011] Furthermore, the silicon dioxide-coated carbon quantum dots are prepared by the following method: (1) using citric acid and ethylenediamine as raw materials, and using a hydrothermal method to prepare a carbon quantum dot solution; (2) using ammonia water, ethyl orthosilicate and the carbon quantum dot solution prepared in step (1) as raw materials, and using Silicon dioxide-coated carbon quantum dots were prepared by the method.
[0012] Furthermore, the silica-coated carbon quantum dots are prepared by the following method: (1) dissolving citric acid and ethylenediamine in deionized water, then heating at 180-220°C for 4-6 hours, and then transferring to a dialysis bag for dialysis for 20-30 hours to prepare a carbon quantum dot solution; (2) adding ammonia water and ethyl orthosilicate to anhydrous ethanol, reacting for 20-40 minutes, and then adding the carbon quantum dot solution prepared in step (1), reacting for 2-3 hours, and then transferring to a dialysis bag for dialysis for 20-30 hours to prepare.
[0013] Furthermore, in step (1), the mass ratio of citric acid to ethylenediamine is 1:1-1.5.
[0014] Furthermore, in step (2), the mass ratio of ammonia water, tetraethyl orthosilicate and carbon quantum dot solution is 1:2-3:1-1.5.
[0015] Furthermore, the molecular weight cut-off of the dialysis bags in steps (1) and (2) is 1000-5000Da.
[0016] The present invention has the following beneficial effects:
[0017] (1) Copper nanoclusters have similar fluorescence responsiveness and spectral tunability as precious metal nanoclusters. They also have broad application prospects due to their abundant sources and low prices. However, nanoclusters formed by single metal copper also have the defects of low fluorescence intensity and poor stability, which makes their sensitivity and reproducibility in bioluminescence detection unsatisfactory. Compared with single metal nanoclusters, the electronic structures and properties of the two metals work synergistically to concentrate the performance advantages of the two metals in the same nanocluster, which can not only improve the stability of single metal nanoclusters but also avoid their exposure. Compared with single copper nanoclusters or gold nanoclusters, copper-gold nanoclusters can form both longer straight chains and dense curved chain structures. This structure can improve the fluorescence intensity of copper-gold nanoclusters, thereby improving the sensitivity of fluorescent probes.
[0018] (2) The present invention constructs a ratiometric fluorescent probe using copper-gold nanoclusters / carbon quantum dots (CuAuNCs / CDs@SiO2). In the CuAuNCs / CDs@SiO2 ratiometric fluorescent probe, both carbon quantum dots and copper-gold nanoclusters can emit fluorescence. CDs@SiO2 hardly reacts with the medium due to the protection of the inert silica coating, thereby providing a stable reference signal. The thiol group of glutathione on the copper-gold nanoclusters has strong reactivity and is greatly affected by the surrounding medium, thereby providing a response signal.
[0019] (3) According to the structure and properties of the target aflatoxin, a fluorescence detection system for aflatoxin based on nanocluster aggregation fluorescence quenching was established. First, Hg 2+ Ions bind to thiol groups, mediating the aggregation of copper-gold nanoclusters, and the fluorescence of the aggregated copper-gold nanoclusters is quenched. After adding aflatoxin, aflatoxin and Hg 2+ A strong complexation occurs, capturing Hg bound to glutathione 2+ ions, thereby disaggregating the aggregated copper-gold nanoclusters and restoring their fluorescence; finally, aflatoxin can be detected based on the degree of fluorescence recovery of the copper-gold nanoclusters.
[0020] (4) The present invention does not require expensive and complex chromatographs, the minimum detection limit of fluorescence detection is 0.56 ng / mL, the linear range is 0-55 ng / mL, the sensitivity is 33.15 mL / ng, the spike recovery is between 99.2% and 105%, and the RSD is less than 5%, which is accurate. At the same time, the RSD of selectivity and anti-interference are 2.2% and 1.1% respectively, so it has certain selectivity and anti-interference.
[0021] (5) The present invention uses a ratiometric fluorescent probe to replace the traditional switch-type fluorescent detection probe, which does not rely on a single signal change and greatly reduces background and environmental errors. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Transmission electron microscopy and hydrated particle size distribution of copper-gold nanoclusters;
[0023] Figure 2 X-ray diffraction pattern and infrared spectrum of copper-gold nanoclusters;
[0024] Figure 3 This is the X-ray photoelectron spectrum of copper-gold nanoclusters;
[0025] Figure 4 The UV spectrum and matrix-assisted laser desorption ionization time-of-flight mass spectrum of copper-gold nanoclusters are shown;
[0026] Figure 5 Schematic diagram of the principle of fluorescence quenching by nanocluster aggregation;
[0027] Figure 6 The transmission electron microscope image and hydrated particle size distribution test image of copper-gold nanoclusters after adding aflatoxin;
[0028] Figure 7 The response of CuAuNCs / CDs@SiO2 ratio probe to different concentrations of aflatoxin;
[0029] Figure 8 To add Hg 2+ Scanning electron microscope images of copper-gold nanoclusters before and after ionization;
[0030] Fig. 9 For different concentrations of Hg 2+ The effect on the fluorescence intensity of CuAuNCs / CDs@SiO2 ratio fluorescence probe;
[0031] Fig.10 The selectivity and anti-interference of CuAuNCs / CDs@SiO2 ratio fluorescence probe for aflatoxin detection. DETAILED DESCRIPTION
[0032] The following examples are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0033] Embodiment 1:
[0034] A method for preparing a copper-gold nanocluster / carbon quantum dot (CuAuNCs / CDs@SiO2) ratio fluorescence probe comprises the following steps:
[0035] (1) Copper-gold nanoclusters (CuAuNCs) were prepared by chemical reduction method using tetrahydrated gold chlorate and dihydrated copper chloride as the main raw materials and glutathione as the ligand. The specific operation was as follows: 0.05mmol CuCl2·2H2O, 0.001mmol HAuCl4·4H2O and 0.92mmol glutathione were dissolved in 5mL ultrapure water respectively. After the CuCl2·2H2O solution and the HAuCl4·4H2O solution were mixed evenly, they were quickly poured into the glutathione solution and stirred for 20min. Then, 1M NaOH solution was added to adjust the pH of the system to 4 and the stirring reaction was continued for 1h. After the reaction was completed, the reaction product was transferred to a centrifuge tube, anhydrous ethanol was added and placed in a centrifuge for high-speed centrifugation (10000rpm, 5min). After centrifugation, the supernatant was discarded, and the precipitate was repeatedly washed with ultrapure water and anhydrous ethanol for 3 times to obtain CuAuNCs, which were then added with anhydrous ethanol and placed in a 4℃ refrigerator for later use.
[0036] (2) 0.42 g of citric acid and 536 μL of ethylenediamine were dissolved in 10 mL of deionized water, and then the solution was transferred to an autoclave lined with polytetrafluoroethylene (Teflon), heated at 200 °C for 5 h, cooled to room temperature after the reaction, and then dialyzed with a cellulose ester membrane bag (mw = 1000 Da) for 24 h to obtain a carbon quantum dot solution, which was then placed in a 4 °C refrigerator for use;
[0037] (3) Add 0.5 mL of ammonia water and 0.2 mL of tetraethyl orthosilicate to 50 mL of ethanol, react for 30 min, then add 1 mL of the carbon quantum dot solution obtained in step (2), stir and react for 2 h, then dialyze with a cellulose ester membrane bag (mw = 3000 Da) for 24 h to obtain silica-coated carbon quantum dots (CDs@SiO2), which are placed in a 4°C refrigerator for later use.
[0038] (4) The CuAuNCs and CDs@SiO2 prepared in steps (1) and (3) were mixed in a volume ratio of 1:4 to obtain a nanostructured carbon nanotube.
[0039] Example 2: Characterization of Copper-Gold Nanoclusters
[0040] (1) The morphology and particle size of the copper-gold nanoclusters prepared in Example 1 were scanned using a transmission electron microscope. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the Cu-Au nanoclusters are spherical in shape and have no obvious lattice arrangement, and their average hydrated particle size is 94.34 nm (PDI = 0.242).
[0041] (2) The copper-gold nanocluster structure prepared in Example 1 was characterized by X-ray diffraction and infrared spectroscopy. Figure 2 As shown. Figure 2It can be seen that the XRD peak width of the copper-gold nanocluster is very large, and the non-sharp diffraction narrow peak indicates that it is an amorphous structure (see Figure 2 a). In the infrared absorption spectrum of copper-gold nanoclusters (see Figure 2 b), SH characteristic stretching vibration peak 2515cm -1 The disappearance of means that a complex is formed between the thiol group of glutathione and copper or gold, and glutathione is successfully bound to the copper-gold nanoclusters to form glutathione-bound copper-gold nanoclusters.
[0042] (3) The elemental composition of the copper-gold nanoclusters prepared in Example 1 was analyzed by X-ray photoelectron spectroscopy. Figure 3 It can be seen that the copper-gold nanoclusters prepared in Example 1 are composed of C, N, O, S, Cu and Au elements. The high-resolution spectrum of Cu 2p (see Figure 3 b) shows the Cu 2p of Cu(0) 1 / 2 and Cu 2p of Cu(Ⅰ) 3 / 2 The peaks of electrons at 951.88eV and 932.28eV, and the characteristic peak of Cu(II) at 942eV were not observed, indicating that there is no Cu(II) in the copper-gold nanoclusters. Figure 3 In c), the characteristic peaks at 84.38 eV and 87.98 eV are considered to be Au 4f 7 / 2 and Au 4f of Au(Ⅰ) 5 / 2 In addition, the S2p high-resolution spectrum (see Figure 3 d) shows two asymmetric peaks at 162.98 eV and 161.98 eV, representing the coordination of S elements with Cu and Au, respectively, which once again confirms the formation of glutathione-bound Cu-Au nanoclusters.
[0043] (4) The copper-gold nanoclusters prepared in Example 1 were analyzed using ultraviolet spectroscopy and matrix-assisted laser desorption ionization time-of-flight mass spectrometry (MALDI-TOF-MS). The results are as follows: Figure 4 As shown. Figure 4 From a, we can see that the copper-gold nanoclusters have an ultraviolet absorption peak at 220nm, which is due to the n-π* electronic transition of Au, and the weak shoulder peak at 270nm is attributed to the LMCT transition; there is no local surface plasmon resonance absorption peak in the visible light region, indicating that no large-sized particles are formed. Figure 4 b shows that the CIE chromaticity coordinates of the copper-gold nanocluster are (0.4620, 0.4923), emitting orange fluorescence. Figure 4 c It can be seen that a peak was observed at m / z 685.4 in the MALDI-TOF-MS spectrum, which may be the [Cu3Au1GSH] molecule.
[0044] Example 3: Detection of aflatoxin using CuAuNCs / CDs@SiO2 ratiometric fluorescent probe
[0045] The core principle of the CuAuNCs / CDs@SiO2 ratiometric fluorescence probe for aflatoxin detection is the fluorescence quenching of nanocluster aggregation. The schematic diagram of the principle is shown in the figure. Figure 5 As shown. 2+ The ion chelates with the two adjacent carbonyl oxygen C=O in the aflatoxin molecule, Hg 2+ It plays the role of a bridge, forming a similar "AFs-Hg 2+ -AFs" structure.Hg 2+ The chelation of ions and carbonyl C=O is very stable, and its binding force is higher than that of Hg 2+ Complexation with glutathione and Hg 2+ With Au + Therefore, aflatoxin and Hg 2+ The formation of ion chelates is the result of competition between aflatoxin and copper-gold nanoclusters for Hg 2+ The result after that, Hg 2+ The Hg-free nanoclusters 2+ Different aflatoxin contents lead to different Hg 2+ Ions are fought out of the copper-gold nanoclusters, which causes different degrees of disaggregation of the copper-gold nanoclusters, resulting in different degrees of fluorescence recovery. Therefore, aflatoxin can be detected based on the change in fluorescence intensity. AFB1, AFB2, AFG1 and AFG2 are the most common derivatives of aflatoxin, and in most cases the mass ratio of AFB1, AFB2, AFG1 and AFG2 is 1.0:0.1:0.3:0.03. The experiment simulated naturally occurring aflatoxin and prepared an aflatoxin solution with a total concentration of 5μg / mL according to the ratio of 1.0:0.1:0.3:0.03. Figure 6 The transmission electron microscope image and hydrated particle size distribution test image of copper-gold nanoclusters after adding aflatoxin. Figure 6 It can be seen that compared with before the addition of aflatoxin, the average hydrated particle size of the copper-gold nanoclusters decreased from 279.3 nm under aggregation to 97.62 nm, and the copper-gold nanoclusters deaggregated instead of further aggregating.
[0046] In order to investigate the response of GSH-CuAuNCs / CDs@SiO2 to aflatoxin, mercuric nitrate solution (mercuric nitrate concentration of 0.75μM, dosage of 500μL) was added to 1mL of CuAuNCs / CDs@SiO2 dispersion, and the fluorescence of copper-gold nanoclusters was quenched. The lowest and most stable fluorescence intensity was detected at 560nm. Then different volumes of aflatoxin solution (concentration of 5μg / mL) were added, and the volume was fixed to 10mL with disodium hydrogen phosphate-potassium dihydrogen phosphate buffer (pH=7.0), so that the equivalent concentrations of aflatoxin were 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 and 65ng / mL, respectively. Mix and shake well, let stand for 30min, excite with a wavelength of 360nm, and record the fluorescence intensity of the maximum emission wavelength at different aflatoxin concentrations. The results are shown in Figure 7 As shown in the figure, as the aflatoxin concentration increases from 0 to 65 ng / mL, the reference signal F1 remains basically constant, while the response signal F2 gradually increases and F1 / F2 gradually decreases. In the range of aflatoxin concentration from 0 to 55 ng / mL, F1 / F2 has a good linear relationship with AFs concentration, and the linear equation is F1 / F2 = -0.0612×C AFs +4.6000(R 2 =0.9986, n=3). According to the calculation formula of the minimum detection limit (LOD): LOD=3SD / k (where SD is the standard deviation of 11 blanks, and k is the slope of the standard curve), the minimum detection limit of the aflatoxin detection method of the present invention is calculated to be 0.56 ng / mL. Similarly, since the reference signal F1 remains basically unchanged, the response signal F2 is proportional to the aflatoxin concentration C AFs Linear fitting was performed, and the absolute value of the slope of the fitting curve was used as the sensitivity of the detection, where the linear equation of the fitting was: F2 = 33.1468 × C AFs +906.3(R 2 =0.9480, n=3). Therefore, the sensitivity of the CuAuNCs / CDs@SiO2 ratiometric fluorescent probe for aflatoxin fluorescence detection is 33.15 mL / ng.
[0047] The above results show that the CuAuNCs / CDs@SiO2 ratio fluorescence probe of the present invention has the advantages of high sensitivity and low detection limit for the detection of aflatoxin.
[0048] Example 4: Hg 2+ Aggregation and fluorescence quenching of Cu-Au nanoclusters mediated by
[0049] Hg 2+ The outer electron configuration is 5s 2 5p 6 5d 10 6s0 , whose empty electron orbital can coordinate with S with lone pair electrons, Hg 2+ -S complexes have sp due to the S symmetry 3 Hybridization forms a regular tetrahedral spatial configuration. In addition, Hg 2+ With Au + The outer d orbitals are filled with 10 electrons, and there is a strong d 10 -d 10 Therefore, Hg 2+ After the addition of Hg 2+ Au + The affinity of Cu-Au nanoclusters can mediate the aggregation of Cu-Au nanoclusters. Figure 8 To add Hg 2+ Electron microscope scanning images of copper-gold nanoclusters before and after ions, by Figure 8 It can be seen that Hg 2+ Aggregation of copper-gold nanoclusters (see Figure 8 a and 8b), and the hydrated particle size tested increased from 59.37 nm to 279.3 nm (see Figure 8 c and 8d).
[0050] Fig. 9 For different concentrations of Hg 2+ (0, 0.15, 0.30, 0.45, 0.60, 0.75, 0.90 μM) on the fluorescence intensity of CuAuNCs / CDs@SiO2 ratio fluorescence probe. The test results show that with the increase of Hg 2+ As the concentration increases, the reference signal F1 remains constant, and the response signal F2 decreases, causing the ratio F1 / F2 to increase. 2+ The aggregation of CuAu nanoclusters caused by Hg addition leads to fluorescence quenching. 2+ After the concentration increased to 0.75 μM, the ratio of F1 / F2 basically did not change. Therefore, 0.75 μM was selected as the Hg 2+ working concentration.
[0051] Example 5: Selectivity and anti-interference ability of CuAuNCs / CDs@SiO2 ratiometric fluorescent probe for aflatoxin detection
[0052] The selectivity and anti-interference of the CuAuNCs / CDs@SiO2 ratio fluorescence probe were investigated by studying its response to other toxins. Ochratoxin (OTA), patulin (PAT), deoxynivalenol (DON), nivalenol (NIV) and zearalenone (ZEN) were selected as interfering substances, with the concentration of each being 50 ng / mL. Fig.10 It can be seen that after adding other substances, the fluorescence intensity ratio F1 / F2 is basically consistent with the blank sample (see Fig.10 The relative standard deviation is 2.2%, indicating that these toxins will not cause the response of the fluorescent probe, and the fluorescent probe has good selectivity. When AFs were added to the above interfering substance standard solution, the fluorescence intensity ratio F1 / F2 of the system decreased significantly, but the F1 / F2 measured in each group was very small (see Fig.10 The relative standard deviation is 1.1%, indicating that the ratio fluorescence probe test system has a good ability to resist interference from other toxins in the detection of AFs.
[0053] Example 6: Accuracy of CuAuNCs / CDs@SiO2 ratiometric fluorescent probe for aflatoxin detection
[0054] The accuracy of the CuAuNCs / CDs@SiO2 ratio fluorescence probe for aflatoxin detection was evaluated by a spike recovery experiment, and the experimental results of the standard addition method are shown in Table 1. As shown in Table 1, the average spike recovery of aflatoxin is between 99.2% and 102.5%, and the RSD is less than 5%. This shows that the CuAuNCs / CDs@SiO2 ratio fluorescence probe of the present invention has high accuracy and potential application value for the detection of aflatoxin.
[0055] Table 1 Determination of aflatoxin by standard addition method
[0056]
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. Application of a copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin, characterized in that: The copper-gold nanocluster / carbon quantum dot ratio fluorescent probe is prepared by the following method: copper-gold nanocluster and silicon dioxide-coated carbon quantum dots are mixed to obtain the probe.
2. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 1, characterized in that: The volume ratio of the copper-gold nanoclusters to the silicon dioxide-coated carbon quantum dots is 1:3-6.
3. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 1, characterized in that: The copper-gold nanoclusters are prepared by the following method: using chloroauric acid and copper salt as raw materials and glutathione as a ligand, and preparing the copper-gold nanoclusters by chemical reduction.
4. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 3, characterized in that: The copper-gold nanoclusters are prepared by the following method: CuCl2·2H2O solution, HAuCl4·4H2O solution and glutathione solution are uniformly mixed and reacted for 20-40 minutes, and then the reaction system is adjusted to acidity and the reaction is continued for 60-90 minutes to obtain the copper-gold nanoclusters.
5. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 4, characterized in that: The molar ratio of the CuCl2·2H2O, the HAuCl4·4H2O and the glutathione is 45-55:1:85-95.
6. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 1, characterized in that: The silicon dioxide-coated carbon quantum dots are prepared by the following method: (1) using citric acid and ethylenediamine as raw materials, and using a hydrothermal method to prepare a carbon quantum dot solution; (2) using ammonia water, ethyl orthosilicate and the carbon quantum dot solution prepared in step (1) as raw materials, and using Silicon dioxide-coated carbon quantum dots were prepared by the method.
7. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 6, characterized in that: The silica-coated carbon quantum dots are prepared by the following method: (1) dissolving citric acid and ethylenediamine in deionized water, then heating at 180-220° C. for 4-6 hours, and then transferring to a dialysis bag for dialysis for 20-30 hours to prepare a carbon quantum dot solution; (2) adding ammonia water and ethyl orthosilicate to anhydrous ethanol, reacting for 20-40 minutes, then adding the carbon quantum dot solution prepared in step (1), reacting for 2-3 hours, and then transferring to a dialysis bag for dialysis for 20-30 hours to prepare.
8. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 7, characterized in that: The mass ratio of the citric acid to the ethylenediamine in step (1) is 1:1-1.
5.
9. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 7, characterized in that: The mass ratio of the ammonia water, the tetraethyl orthosilicate and the carbon quantum dot solution in step (2) is 1:2-3:1-1.
5.
10. The use of the copper-gold nanocluster / carbon quantum dot ratiometric fluorescent probe in detecting aflatoxin according to claim 7, characterized in that: The molecular weight cut-off of the dialysis bags in steps (1) and (2) is 1000-5000Da.
Citation Information
Patent Citations
Dual emission rate type fluorescent probe for visually detecting carbon dots-Au nanoclusters of mercury ions and preparation method
CN105067577A
CDs / SiO2 / AuNCs ratiometric fluorescent probe, preparation method and application
CN109609125A
Method for preparing nanohybrid capable of being simultaneously used in ratio fluorescence sensing and ratio electrochemical sensing
CN109856101A
Cited By
Bimetallic copper-gold nano-cluster Cu / AuNCs-coated ESM and synthetic method and application thereof
CN120133534A
Ratio-type fluorescent probe and application thereof in distinguishing and detecting aflatoxin B1 and aflatoxin B2a
CN121592340A