Method and device for RH refining of ultra-low carbon steel

By using a bottom blowing gun to blow into specific gases and adjusting gas flow during RH vacuum smelting ultra-low carbon steel, the problem of controlling the carbon content of the liquid steel is solved, and the effect of efficient decarbonization and shortening the refining cycle is achieved, which improves production efficiency and Product quality.

CN118910364APending Publication Date: 2024-11-08CHINA NAT HEAVY MACHINERY RES INSTCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964760.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the RH vacuum smelting ultra-low carbon steel, it is difficult to effectively control the carbon content of the molten steel, especially when the carbon content is less than 10 ppm, the conventional process has the problem of long time consumption and it is difficult to achieve the best in different refining stages. Decarbonization effect and molten steel circulation efficiency.

Method used

Adjust the gas flow and pressure to accelerate the liquid steel by using a bottom blower vertically injecting the high-speed O2, CO2, H2, Ar, N2 single-component or multi-component airflow at different stages of RH vacuum refining ultra-low carbon steel. Flow and decarbonization reactions ensure optimal decarbonization and molten steel circulation efficiency at each stage.

Benefits of technology

The decarbonization efficiency is significantly improved, the metallurgical reaction and degassing time is shortened, the carbon content in the molten steel is stably controlled below 10ppm, and the refining cycle is shortened by 1-3 minutes, which improves production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910364A_ABST
    Figure CN118910364A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of circulation control of ultra-low carbon steel smelting molten steel, and discloses an RH refining ultra-low carbon steel method and device. In each stage of refining, high-speed single-component or multi-component airflow such as Ar, O2, CO2, H2 and N2 is vertically and upwards blown in through a bottom blowing gun, the kinetic energy of upward flowing of molten steel and the molten steel flow of an effective reaction layer are effectively improved, and the purpose of improving the quality of the molten steel is achieved. Therefore, the decarburization efficiency is obviously improved. The invention further provides an RH refining ultra-low carbon steel device which comprises a vacuum chamber arranged above a steel ladle, a dip pipe is arranged at the lower end of the vacuum chamber and comprises an ascending pipe and a descending pipe, and the ascending pipe and the descending pipe are inserted into molten steel in the steel ladle. And the multiple bottom blowing guns are uniformly arranged on at least one row of the periphery of the outer wall of the ascending pipe in an arc shape in the circumferential direction of the ascending pipe, the carbon content in molten steel can be stably controlled to be 10 ppm or below, the refining period is shortened by 1-3 min, and powerful technical support is provided for efficient and low-cost production of ultra-low carbon steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of molten steel circulation control for ultra-low carbon steel smelting, and in particular to a method and device for RH refining ultra-low carbon steel. Background Art

[0002] Ultra-low carbon steel is the main material for complex automotive stamping parts. With the rapid development of the automotive industry, it not only requires higher cleanliness, but also increasingly pursues lower target carbon content in steel. At present, the key link in the production of ultra-low carbon steel is the RH vacuum smelting technology. The RH vacuum smelting technology specifically involves inserting an immersion tube into the molten steel. The molten steel enters the vacuum chamber from the riser and falls back into the ladle from the downcomer due to gravity. The molten steel completes most of the metallurgical reactions in the vacuum chamber, including decarburization reactions.

[0003] However, in the process of RH vacuum smelting of ultra-low carbon steel, as the carbon content in the molten steel decreases, the vacuum environment only has a significant effect on the decarburization reaction of the upper surface reaction layer of the molten steel in the vacuum chamber, while the decarburization reaction in the middle and lower parts of the molten steel in the vacuum chamber almost stops. The final carbon content of the molten steel is difficult to effectively and stably control below 20ppm. Therefore, there are certain difficulties in smelting ultra-low carbon steel using the conventional RH process. For steels with a production target carbon content of less than 10ppm, it takes longer and is more difficult to complete.

[0004] Therefore, in the process of RH vacuum refining of ultra-low carbon steel, how to control the gas flow and pressure blown into the bottom blowing gun to ensure the best decarburization effect and steel liquid circulation efficiency in different refining stages is an urgent problem to be solved. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method and device for RH refining ultra-low carbon steel, in which high-speed O is blown vertically upward through a bottom blowing gun at different stages of RH vacuum refining ultra-low carbon steel refining start, decarburization initial stage, decarburization stable stage, steel liquid circulation stage and refining end. 2 , CO 2 , H 2 , Ar, N 2 The single-component or multi-component gas flow accelerates the kinetic energy of the molten steel flowing upward, increases the molten steel flow rate in the effective reaction layer, enhances the ability to remove carbon from the molten steel, and shortens the time consumed by metallurgical reaction and degassing. It can stably and quickly control the terminal carbon content in the molten steel to below 10ppm, and the refining cycle can be shortened by 1-3 minutes. The control of the gas flow rate and pressure blown into the bottom blowing gun is solved to ensure the best decarburization effect and molten steel circulation efficiency at different refining stages.

[0006] In a first aspect, the present invention provides a method for RH refining ultra-low carbon steel, comprising the following steps: S1, initial state, the gas blown into the bottom blowing gun is N2 , gas flow rate is Q 1 ; S2, refining starts, when the immersion tube contacts the liquid surface of the molten steel, the blowing gas of the bottom blowing gun is switched to a gas containing Ar, O 2 , CO 2 , H 2 The gas flow rate of one or more components is Q 1 ; S3, enter the rapid decarburization period, after the immersion tube is inserted into the molten steel, vacuum is started, and the molten steel begins to circulate in the vacuum chamber and the ladle. The type of gas blown into the bottom blowing gun is the same as in S2, and the gas flow rate is Q 2 , vacuum time is 0-6min; S4, after vacuum refining for 6 minutes, sampling is performed to analyze the sample components to obtain the carbon content; S5, enter the decarburization stable period, the gas blown into the bottom blowing gun is switched to Ar, and the gas flow rate is Q 3 , vacuum refining time is 7-20min; S6, when vacuum refining is carried out to the interval of 11-20 minutes, sampling operation is carried out to test the sample composition. If the carbon content meets the target carbon content requirement of the steel grade, the process proceeds to S7; S7, enter the molten steel circulation period, the gas blown into the bottom blowing gun is Ar, and the gas flow rate is Q 4 After adjusting the alloy composition and the temperature of the molten steel, if the temperature is measured and the sampling is qualified, the vacuum chamber is broken to end the refining; S8. After refining, the immersion tube of the vacuum chamber is separated from the liquid surface of the molten steel, and the blowing gas of the bottom blowing gun is switched to N 2 , gas flow rate is Q 5 , Q 5 =Q 1 .

[0007] Furthermore, the gas flow rate blown into the bottom blowing gun is specifically:

[0008] Where: Q is the total gas flow rate of the bottom blowing gun, Nm 3 / h; is the correction coefficient, with a value range of 0.5-1.5; D is the diameter of the spray gun outlet, mm; V is the spray gun outlet velocity, m / s; ΔP is the pressure difference between the gas source pressure and the vacuum chamber, MPa; n is the number of bottom blowing spray guns.

[0009] Furthermore, during the process from the initial state to the end of refining, the outlet pressure of the bottom blowing gun is ≥0.2MPa; Furthermore, the gas flow rate of the bottom blowing gun is Q 3 =ƞ×Q 2=ε×Q 4 =τ × Q 1 , where ƞ takes the value of 1.5-2.5, ε takes the value of 3.5-4.5, and τ takes the value of 6.0-7.0.

[0010] Furthermore, the vacuum degree in the rapid decarburization period in S3 reaches less than 100 Pa within 3 minutes.

[0011] Furthermore, the outlet of the bottom blowing gun is arranged below the liquid level of the molten steel in the vacuum chamber, and the gas blown into the bottom blowing gun directly enters the interior of the molten steel in the vacuum chamber.

[0012] In the second aspect, the present invention also provides an RH refining ultra-low carbon steel device, which is applied to the above-mentioned RH refining ultra-low carbon steel method, including a vacuum chamber arranged above the ladle, an immersion pipe is arranged at the lower end of the vacuum chamber, the immersion pipe includes a riser and a downcomer, the riser and the downcomer are inserted into the molten steel in the ladle, and a plurality of bottom blowing guns are evenly arranged in an arc shape in at least one row around the outer wall of the riser along the circumferential direction of the riser, the inlet of the bottom blowing gun is connected to the gas source pipeline, and the outlet thereof is arranged at the bottom of the vacuum chamber.

[0013] Furthermore, the number of the bottom blowing guns is 1-12.

[0014] Furthermore, the bottom blowing guns are evenly distributed in an arc shape in 1-3 rows along the circumferential direction of the riser and are arranged around the outer wall of the riser.

[0015] Furthermore, the outlet diameter of the bottom blowing gun is 2-10 mm, the inlet of the bottom blowing gun is connected to the gas source pipeline, and the gas source of the gas source pipeline includes O 2 , CO 2 , Ar, H 2 、N 2 , the gas source pressure is 0.4-1.6MPa.

[0016] The beneficial effects of the present invention are: The decarburization efficiency is significantly improved: by using the bottom blowing gun technology, the flow of molten steel is accelerated by blowing in specific gases and controlling the gas flow, thereby enhancing the decarburization capacity and stably controlling the carbon content in the molten steel below 10ppm.

[0017] Shortened refining cycle: Optimizing the decarburization process reduces metallurgical reaction and degassing time, shortening the refining cycle by 1-3 minutes compared with conventional methods and improving production efficiency.

[0018] Improved product quality: Precise control of gas flow and flow ensures reaction stability, which in turn improves product quality and uniformity.

[0019] Strong flexibility and scalability: The method and device can be adjusted according to different smelting requirements and are suitable for the production of various steel grades.

[0020] Reduced production risks: Optimizing the refining process reduces the risk of incomplete metallurgical reactions or poor degassing effects, and enhances production safety.

[0021] In general, the present invention has a positive driving effect on the steel smelting industry, not only improving the decarbonization efficiency and product quality, but also shortening the refining cycle and reducing production risks. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a flow chart of a method for RH refining ultra-low carbon steel; Figure 2 It is a schematic diagram of the structure of a RH refining ultra-low carbon steel device; Figure 3 The present invention is a cross-sectional view of an embodiment of a vacuum chamber of an RH refining ultra-low carbon steel apparatus.

[0023] Among them, 1. vacuum chamber; 2. ladle; 3. riser; 4. bottom blowing gun; 5. downcomer; 6. molten steel. DETAILED DESCRIPTION

[0024] The following is combined with Figures 1 to 3 The preferred embodiments of the present invention are described in detail so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0025] like Figure 1 As shown, the present invention provides a method for RH refining ultra-low carbon steel, comprising the following steps: In step S1, in the initial state, the gas blown into the bottom blowing gun is N 2 , gas flow rate is Q 1 ; Function and effect of step S1: Before refining begins, the gas blown into the bottom blowing gun is N2, and the gas flow rate is Q1. The purpose of this step is to create a relatively stable initial environment for the refining process. As an inert gas, N2 will not affect the composition of the molten steel, which is conducive to the smooth progress of the subsequent refining process.

[0026] In step S2, when refining starts and the immersion tube contacts the liquid surface of the molten steel, the blowing gas of the bottom blowing gun is switched to a gas containing Ar, O 2 , CO 2 , H 2 The gas flow rate of one or more components is Q 1 ; Step S2 function and effect: When the immersion tube contacts the liquid surface of the molten steel, the gas blown into the bottom blowing gun is switched to a gas flow containing one or more components of Ar, O2, CO2, and H2, and the gas flow rate remains Q1. This step begins to introduce refining gases with specific functions, such as Ar for degassing, O2 and CO2 for oxidative decarburization, etc. By changing the gas composition, it prepares for the subsequent decarburization and refining process.

[0027] In step S3, the rapid decarburization period begins, and the vacuum degree reaches less than 100 Pa within 3 minutes. After the immersion tube is inserted into the molten steel, vacuuming begins, and the molten steel begins to circulate in the vacuum chamber and the ladle. The type of gas blown into the bottom blowing gun is the same as that in S2, and the gas flow rate is Q 2 , vacuum time is 0-6min; The rapid decarburization period refers to the stage in the RH vacuum refining of ultra-low carbon steel when the immersion tube is inserted into the molten steel and vacuum is started, and the molten steel circulates in the vacuum chamber and the ladle. In this stage, the flow and mixing of the molten steel are accelerated by increasing the gas flow and vacuuming operation, thereby accelerating the decarburization reaction and effectively reducing the carbon content in the molten steel.

[0028] Step S3: After the immersion tube is inserted into the molten steel, vacuuming begins and the molten steel begins to circulate in the vacuum chamber and the ladle. At this time, the type of gas blown into the bottom blowing gun is the same as that in S2, but the gas flow rate is increased to Q 2 , the vacuum time is 0-6min. During the rapid decarburization period, by increasing the gas flow and vacuuming operation, the fluidity and mixing effect of the molten steel can be significantly improved, the carbon removal process can be accelerated, and a higher vacuum degree (less than 100Pa) can be achieved, which is conducive to the escape of gas in the molten steel.

[0029] In step S4, after the vacuum smelting lasts for 6 minutes, sampling is performed to analyze the sample components to obtain the carbon content; Step S4: When the vacuum smelting is carried out for 6 minutes, sampling is carried out to test the sample composition to obtain the carbon content. This step is to monitor the carbon content change in the molten steel in real time to ensure that the refining process is carried out according to the predetermined target.

[0030] In step S5, the decarburization enters the stable period, and the gas blown into the bottom blowing gun is switched to Ar, and the gas flow rate is Q 3 , vacuum refining time is 7-20min; The decarburization stable period refers to a stage in which the decarburization reaction of the molten steel is relatively stable after the rapid decarburization period during the RH vacuum refining of ultra-low carbon steel. In this stage, the carbon content in the molten steel begins to stabilize and the decarburization reaction rate slows down. In order to maintain the decarburization efficiency and the smooth progress of the reaction, the bottom blowing gun will switch to blowing Ar gas, and by adjusting the gas flow and vacuum refining time, the carbon content in the molten steel will be further reduced to the target value, in preparation for entering the molten steel circulation period.

[0031] Step S5: After entering the decarburization stable period, the gas blown into the bottom blowing gun is switched to Ar, and the gas flow rate is Q 3 The addition of Ar helps to further remove gases such as hydrogen and nitrogen from the molten steel. In this stage, the stable gas flow and gas type are used to ensure the smooth progress of the decarburization process.

[0032] In step S6, when the vacuum refining is performed for 11-20 minutes, sampling is performed to test the sample composition. If the carbon content meets the target carbon content requirement of the steel grade, the process proceeds to S7; Step S6 Function and Effect: When vacuum refining reaches the interval of 11-20min, sampling is performed again to test the sample composition. If the carbon content meets the target carbon content requirement of the steel grade, the next step is entered. This step is to confirm whether the carbon content in the molten steel reaches the refining target and ensure product quality.

[0033] In step S7, the steel liquid circulation period begins, the gas blown into the bottom blowing gun is Ar, and the gas flow rate is Q 4 After adjusting the alloy composition and the temperature of the molten steel, if the temperature is measured and the sampling is qualified, the refining is completed; Step S7: After entering the steel liquid circulation period, the bottom blowing gun continues to blow Ar, and the gas flow rate is Q 4 At this time, the alloy composition and molten steel temperature are mainly adjusted to ensure that the molten steel composition and temperature meet the product requirements. After the adjustment is completed, the temperature measurement and sampling operation is carried out. If it is qualified, the vacuum chamber is broken and the smelting is ended.

[0034] In step S8, after refining is completed, the immersion tube of the vacuum chamber is separated from the liquid surface of the molten steel, and the blowing gas of the bottom blowing gun is switched to N 2 , gas flow rate is Q 5 , Q 5 =Q 1 .

[0035] Step S8: After refining, the immersion tube of the vacuum chamber is separated from the liquid surface of the molten steel, and the blowing gas of the bottom blowing gun is switched back to N2. 2 , gas flow rate is Q 5 , Q 5 =Q 1This step is to end the refining process and ensure that the refining equipment is properly protected and ready for the next refining process.

[0036] Specifically, the gas flow rate blown into the bottom blowing gun is:

[0037] Where: Q is the total gas flow rate of the bottom blowing gun, Nm 3 / h; is the correction coefficient, with a value range of 0.5-1.5; D is the diameter of the spray gun outlet, mm; V is the spray gun outlet velocity, m / s; ΔP is the pressure difference between the gas source pressure and the vacuum chamber, MPa; n is the number of bottom blowing spray guns.

[0038] From the initial state to the end of refining, the outlet pressure of the bottom blowing gun is ≥0.2MPa; The gas flow rate of the bottom blowing gun is Q 3 =ƞ×Q 2 =ε×Q 4 =τ × Q 1 , where ƞ takes the value of 1.5-2.5, ε takes the value of 3.5-4.5, and τ takes the value of 6.0-7.0.

[0039] The outlet of the bottom blowing gun is arranged below the liquid level of the molten steel in the vacuum chamber, and the gas blown into the bottom blowing gun directly enters the interior of the molten steel in the vacuum chamber.

[0040] like Figure 2As shown, the present invention also provides an RH refining ultra-low carbon steel device, which is applied to the above-mentioned RH refining ultra-low carbon steel method, including a vacuum chamber 1 arranged above the ladle 2, an immersion pipe is arranged at the lower end of the vacuum chamber 1, the immersion pipe includes an ascending pipe 3 and a descending pipe 5, the ascending pipe 3 and the descending pipe 5 are inserted into the molten steel 6 in the ladle 2, and multiple bottom blowing guns 4 are evenly arranged in multiple layers around the outer wall of the ascending pipe 3 along the circumferential direction of the ascending pipe 3, the inlet of the bottom blowing gun 4 is connected to the gas source pipeline, and the outlet thereof is arranged at the bottom of the vacuum chamber 1. The molten steel 6 in the ladle 2 enters the vacuum chamber 1 from the riser 3, and falls back into the ladle 2 from the downcomer 5. The corresponding gas types and matching gas flow rates are blown in through the bottom blowing gun 4 at different stages of vacuum refining, namely, the beginning of refining, the rapid decarburization period, the decarburization stable period, the molten steel circulation period, and the end of refining, so that the flow rate of the molten steel 6 in the upper part (i.e., the reaction layer) of the molten steel 6 in the vacuum chamber 1 is increased, the decarburization efficiency is significantly improved, the limit carbon content under the conventional RH process can be further reduced, the carbon content in the molten steel 6 can be stably removed to below 10 ppm, and at the same time, the time consumed by the metallurgical reaction and degassing is shortened, and the refining cycle can be shortened by 1-3 minutes, thereby reducing the production cost of ultra-low carbon steel. The number of bottom blowing guns 4 is 1-12, and the bottom blowing guns 4 are evenly distributed in 1-3 circles along the circumferential direction of the riser 3 and are arranged around the outer wall of the riser 3. The outlet diameter of the bottom blowing gun 4 is 2-10 mm, and the inlet of the bottom blowing gun 4 is connected to the gas source pipeline. The gas source of the gas source pipeline includes O2, CO2, Ar, H2, N2, and the gas source pressure is 0.4-1.6 MPa.

[0041] Embodiment 1: In this embodiment, the bottom blowing guns are evenly arranged around the riser in one circle, the total number of bottom blowing guns is 7, the bottom blowing gun outlet diameter is 4 mm, the bottom blowing gun inlet is connected to the gas source valve station, and the gas source types include O 2 , CO 2 , Ar, H 2 、N 2 , the pressure of the gas source valve station is 0.9 MPa. Under the above settings, specifically, a method for RH refining ultra-low carbon steel comprises the following steps: S1, initial state, the gas blown into the bottom blowing gun is N 2 , gas flow rate is Q 1 =98Nm 3 / h; S2. At the beginning of refining, when the immersion tube contacts the liquid surface of the molten steel, the gas blown into the bottom blowing gun is N 2 Switch to Ar and H 2 Mixed gas, gas flow rate Q 1 =98Nm 3 / h; S3, rapid decarburization period, the vacuum degree of the vacuum chamber reaches 50Pa in 2.5min, the vacuum time is 0-6min, after the immersion tube is inserted into the molten steel to a certain depth, vacuuming begins, the molten steel begins to circulate in the vacuum chamber and the ladle, and the gas flow rate Q 2 =315Nm 3 / h; S4. When vacuum refining is 6 minutes, sampling is performed and the sample composition is tested. The carbon content is 22ppm. S5, enter the decarburization stable period, the vacuum refining time is 7min-20min, the gas blown into the bottom blowing gun is switched to Ar, and the gas flow rate is Q 3 =630Nm 3 / h, S6. When vacuum refining is carried out for 11-20 minutes, sampling is performed to test the sample composition. The carbon content is 12ppm, which meets the target carbon content requirement of the steel grade. S7, enter the molten steel circulation period, after the target carbon content of the steel grade in S6 meets the requirements, the gas blown into the bottom blowing gun is Ar, and the total gas flow rate is Q 4 =155Nm 3 / h, after the alloy composition and temperature are adjusted, temperature measurement and sampling are carried out, and refining is ended by breaking the air; S8, after refining is completed, the vacuum chamber is broken, the immersion tube of the vacuum chamber is separated from the liquid surface of the molten steel, and the gas blown into the bottom blowing gun is switched to N 2 , the total gas flow is Q 5 98Nm 3 / h.

[0042] The gas flow rate Q of the bottom blowing gun is adjusted according to the formula:

[0043] Where Q is the total gas flow rate of the bottom blowing gun, Nm 3 / h; is the correction coefficient, with a value range of 0.5-1.5; D is the diameter of the spray gun outlet, mm; V is the spray gun outlet velocity, with a value of (30-300) m / s; ΔP is the pressure difference between the gas source pressure and the vacuum chamber pressure, MPa; n is the number of bottom blowing spray guns.

[0044] Embodiment 2: In this embodiment, the bottom blowing guns are evenly arranged around the riser for 2 circles, the total number of bottom blowing guns is 10, the bottom blowing gun outlet diameter is 3 mm, the bottom blowing gun inlet is connected to the gas source valve station, and the gas source types include O 2 , CO 2 , Ar, H 2 、N 2, the pressure of the gas source valve station is 0.9 MPa. Under the above settings, specifically, a method for RH refining ultra-low carbon steel comprises the following steps: S1, initial state, the gas blown into the bottom blowing gun is N 2 , gas flow rate is Q 1 =76Nm 3 / h; S2. At the beginning of refining, when the immersion tube contacts the steel liquid surface, the gas blown into the bottom blowing gun is N 2 Switch to Ar and CO 2 Mixed gas, gas flow rate Q 1 =76Nm 3 / h; S3, rapid decarburization period, the vacuum degree of the vacuum chamber reaches 50Pa in 2.5min, the vacuuming time is 0-6min, after the immersion tube is inserted into the molten steel to a certain depth, vacuuming begins, the molten steel begins to circulate in the vacuum chamber and the ladle, and the gas flow rate Q 2 =250Nm 3 / h, S4. When vacuum refining is 6 minutes, sampling is performed and the sample composition is tested. The carbon content is 22ppm. S5, decarburization stable period, vacuum refining time is 7min-20min. The gas blown into the bottom blowing gun is switched to Ar, and the total gas flow is Q 3 =500Nm 3 / h, S6. When vacuum refining is carried out for 11-20 minutes, sampling is performed to test the sample composition. The carbon content is 12ppm, which meets the target carbon content requirement of the steel grade. S7, enter the molten steel circulation period, after the target carbon content of the steel grade in S6 meets the requirements, the gas blown into the bottom blowing gun is Ar, and the total gas flow rate is Q 4 =130Nm 3 / h, after the alloy composition and temperature adjustment are completed, the temperature measurement and sampling operation is carried out, and the refining can be ended; S8, after refining is completed, the vacuum chamber is broken, the vacuum chamber immersion tube is separated from the liquid surface of the molten steel, and the gas blown into the bottom blowing gun is switched to N 2 , the total gas flow is Q 5 76Nm 3 / h.

[0045] The present invention allows the molten steel in the ladle to enter the vacuum chamber from the ascending pipe, fall back into the ladle from the descending pipe, and then pass through the bottom blowing gun arranged at the lower end of the vacuum chamber to blow high-speed oxygen into the interior of the vacuum chamber at different stages of vacuum refining, such as the beginning of refining, the initial stage of decarburization, the stable stage of decarburization, the circulation stage of molten steel, and the end of refining. 2 , CO 2 , H2 , Ar, N 2 The single-component or multi-component gas flow and the matching gas flow accelerate the kinetic energy of the molten steel flowing upward, that is, the molten steel flow in the effective reaction layer is increased, and the decarburization efficiency is significantly improved. The limit carbon content under the conventional RH process can be further reduced, and the carbon content in the molten steel can be stably removed to below 10ppm. At the same time, the time consumed by metallurgical reaction and degassing is shortened, and the refining cycle can be shortened by 1-3 minutes, thereby reducing the production cost of ultra-low carbon steel.

[0046] The present invention solves the technical problem of controlling the gas flow rate and pressure blown into the bottom blowing gun to ensure the best decarburization effect and steel liquid circulation efficiency in different refining stages by the following methods: First, the present invention designs a gas flow control strategy. At different stages of refining, the gas flow of the bottom blowing gun is adjusted according to demand. For example, in the rapid decarburization period, the kinetic energy of the upward flow of molten steel is accelerated by increasing the gas flow, and the molten steel flow in the reaction layer is increased, thereby enhancing the decarburization capacity. In the decarburization stable period and the molten steel circulation period, the flow is adjusted according to the smelting process to maintain a stable decarburization efficiency and molten steel circulation efficiency.

[0047] Secondly, the present invention also focuses on pressure control to ensure that the outlet pressure of the bottom blowing gun is always maintained at a certain level (≥0.2MPa), so that the gas can be blown into the molten steel stably and efficiently, further promoting the circulation of the molten steel and the decarburization reaction.

[0048] Finally, according to the requirements of different refining stages, the present invention selects different types of gases or gas combinations for blowing to further optimize the decarburization effect and the circulation efficiency of the molten steel.

[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for RH refining ultra-low carbon steel, characterized in that: The following steps are involved: S1, initial state, the gas blown into the bottom blowing gun is N2, and the gas flow rate is Q1; S2, when refining starts and the immersion tube contacts the liquid surface of the molten steel, the blowing gas of the bottom blowing gun is switched to a gas flow containing one or more components of Ar, O2, CO2, and H2, and the gas flow rate is Q1; S3, enter the rapid decarburization period, after the immersion tube is inserted into the molten steel, vacuuming begins, and the molten steel begins to circulate in the vacuum chamber and the ladle. The type of gas blown into the bottom blowing gun is the same as that in S2, the gas flow rate is Q2, and the vacuuming time is 0-6min; S4. After vacuum refining for 6 minutes, take samples and analyze the sample components to obtain the carbon content; S5, entering the decarburization stable period, the gas blown into the bottom blowing gun is switched to Ar, the gas flow rate is Q3, and the vacuum refining time is 7-20min; S6, when the vacuum refining is carried out to the interval of 11-20 minutes, sampling operation is carried out to test the sample composition. If the carbon content meets the target carbon content requirement of the steel grade, the process proceeds to S7; S7, entering the molten steel circulation period, the gas blown into the bottom blowing gun is Ar, the gas flow rate is Q4, the alloy composition and molten steel temperature are adjusted, and the temperature measurement and sampling are qualified, and the vacuum chamber is broken, and the refining is ended; S8. After refining, the immersion tube of the vacuum chamber is separated from the liquid surface of the molten steel, and the blowing gas of the bottom blowing gun is switched to N2, and the gas flow rate is Q5, Q5=Q1.

2. The method for RH refining of ultra-low carbon steel according to claim 1, characterized in that: The gas flow rate blown into the bottom blowing gun is specifically: ; Where: Q is the total gas flow rate of the bottom blowing gun, Nm 3 / h; is the correction coefficient, with a value range of 0.5-1.5; D is the diameter of the spray gun outlet, mm; V is the spray gun outlet velocity, m / s; ΔP is the pressure difference between the gas source pressure and the vacuum chamber, MPa; n is the number of bottom blowing spray guns.

3. The method for RH refining of ultra-low carbon steel according to claim 1, characterized in that: During the process from the initial state to the end of refining, the outlet pressure of the bottom blowing gun is ≥0.2MPa.

4. The method for RH refining of ultra-low carbon steel according to claim 1, characterized in that: The relationship between the gas flow rates blown in by the bottom blowing gun is Q3=ƞ×Q2=ε×Q4=τ×Q1, where ƞ takes a value of 1.5-2.5, ε takes a value of 3.5-4.5, and τ takes a value of 6.0-7.

0.

5. The method for RH refining of ultra-low carbon steel according to claim 1, characterized in that: The vacuum degree during the rapid decarburization period in S3 reaches less than 100 Pa within 3 minutes.

6. The method for RH refining of ultra-low carbon steel according to claim 1, characterized in that: The outlet of the bottom blowing gun is arranged below the liquid level of the molten steel in the vacuum chamber, and the gas blown into the bottom blowing gun directly enters the interior of the molten steel in the vacuum chamber.

7. An RH refining ultra-low carbon steel device, applied to the above-mentioned RH refining ultra-low carbon steel method, characterized in that: The invention comprises a vacuum chamber (1) arranged above a ladle (2), a dip tube being arranged at the lower end of the vacuum chamber (1), the dip tube comprising an ascending tube (3) and a descending tube (5), the ascending tube (3) and the descending tube (5) being inserted into the molten steel (6) in the ladle (2), a plurality of bottom blowing guns (4) being arranged in at least one row in an arc shape uniformly along the circumferential direction of the ascending tube (3) around the outer wall of the ascending tube (3), the inlet of the bottom blowing gun (4) being connected to a gas source pipeline, and the outlet thereof being arranged at the bottom of the vacuum chamber (1).

8. The RH refining ultra-low carbon steel device according to claim 7, characterized in that: The number of the bottom blowing guns (4) is 1-12.

9. The RH refining ultra-low carbon steel device according to claim 7, characterized in that: The bottom blowing guns (4) are evenly distributed in an arc shape in 1 to 3 rows along the circumferential direction of the riser (3), and are arranged around the outer wall of the riser (3).

10. The RH refining ultra-low carbon steel device according to claim 7, characterized in that: The outlet diameter of the bottom blowing gun (4) is 2-10 mm, and the inlet of the bottom blowing gun (4) is connected to a gas source pipeline. The gas source of the gas source pipeline includes O2, CO2, Ar, H2, and N2, and the gas source pressure is 0.4-1.6 MPa.