Method for enhanced bioleaching of chalcopyrite
By adding monovalent copper ion complexing agent to the chalcopyrite biological leaching system and controlling the potential and iron concentration, the problem of insufficient chalcopyrite leaching rate is solved, and efficient oxidation leaching and low-cost copper leaching effects are achieved.
Patent Information
- Application Number
- CN202410629385.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively regulate the leaching environment of chalcopyrite, resulting in insufficient copper leaching rate and selective dissolution of non-copper sulfide minerals, making it difficult to improve the biological leaching effect.
By adding monovalent copper ion complexing agent to the chalcopyrite biological leaching system, the redox potential and iron concentration of the solution are coordinated and controlled within the range of 580-650mV and 2-5g/L, the oxidation of chalcopyrite and Microbial activity reduces the degradation rate of leaching enhancer.
The efficient oxidative leaching of chalcopyrite was achieved, and the copper leaching rate reached more than 82.8%, reducing the dissolution and acid production of non-copper sulfide minerals, reducing the burden of iron removal and acid removal, and low consumption of enhancement agents and low cost.
Smart Images

Figure CN118910406A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biometallurgy, and relates to a leaching method of chalcopyrite, in particular to a method for enhanced bioleaching of chalcopyrite. Background Art
[0002] Biometallurgy technology is generally used for leaching of sulfide minerals, and the main processes include bio-heap leaching, bio-agitation leaching, etc. Biometallurgy technology is used for leaching of sulfide copper ores. The process is to promote the oxidation of copper minerals by oxidizing divalent iron and reducing sulfur through the action of microorganisms. However, due to the high lattice energy of chalcopyrite, it is difficult to control the potential during the leaching process, and the microbial activity is insufficient, resulting in insufficient copper leaching rate, so the industrial application of chalcopyrite ore bioleaching is difficult.
[0003] In the prior art, additives are usually added to the leaching system to enhance the leaching of chalcopyrite.
[0004] CN103993171A discloses a method for promoting chalcopyrite bioleaching by adding a nonionic surfactant. The method adopts the method of adding a nonionic surfactant polyethylene glycol to the leaching solution to improve the bioleaching effect. The polyethylene glycol can increase the concentration of the microorganisms used in the leaching system without adding ferrous iron, and can weaken the wrapping of the passivation layer in the leaching system with adding ferrous iron, thereby improving the leaching efficiency.
[0005] CN105861823A discloses a method for strengthening the microbial leaching of chalcopyrite. In this method, pyrite and sphalerite are added to the leaching system, and the oxidation decomposition of chalcopyrite is strengthened by controlling the pH of the solution to be low and maintaining a high iron ion concentration and potential, thereby improving the leaching rate of copper.
[0006] CN115287453A discloses a method for enhancing chalcopyrite bioleaching by using a flotation collector. Adding potassium amyl xanthate collector can reduce the surface tension of the solution and the formation of passivation products, thereby improving the bioleaching of copper.
[0007] CN110352256A discloses a process for leaching metal sulfides using a reagent having a thiocarbonyl functional group. The method comprises contacting the metal sulfide with an acidic sulfate solution containing iron sulfate and a reagent having a thiocarbonyl functional group to produce a rich solution containing metal ions. However, the process does not take into account the problem of microbial activity and the potential of the chalcopyrite reaction, nor does it consider the problem of controlling the degradation of the thiocarbonyl functional group reagent. In particular, under uncontrolled potential, the degradation of the reagent increases significantly after the potential increases.
[0008] In the actual bioleaching process of chalcopyrite, its leaching environment is an extremely complex system, which involves many factors such as pH, redox potential, microbial activity, and iron ion concentration of the leaching system. The system potential cannot be regulated in the traditional bio-heap leaching process, and the leaching rate of chalcopyrite cannot be guaranteed. At the same time, the dissolution of other sulfide minerals cannot be controlled, and the selective leaching of chalcopyrite cannot be achieved. The prior art lacks reasonable coordinated regulation of its complex solution environment, so it is difficult to further improve the bioleaching effect of copper. Therefore, it is necessary to provide a method for enhanced bioleaching of chalcopyrite. Summary of the invention
[0009] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for enhanced bioleaching of chalcopyrite, while solving the three problems of chemical reaction kinetics, potential window and microbial activity that limit the oxidation efficiency of chalcopyrite, and effectively improving the bioleaching efficiency of chalcopyrite.
[0010] To achieve this object, the present invention adopts the following technical solutions:
[0011] The present invention provides a method for enhanced bioleaching of chalcopyrite, the method comprising:
[0012] The chalcopyrite ore, the microbial leaching extract and the leaching enhancer are mixed and leached to obtain a leaching solution;
[0013] The microbial leaching extract is an acidic ferric iron solution containing acidophilic oxidizing microorganisms;
[0014] During the leaching process, the redox potential of the solution of the leaching system is controlled to be 580-650 mV (vs. SHE), and the iron concentration in the solution is controlled to be 2-5 g / L.
[0015] The enhanced leaching method provided by the present invention comprises adding a monovalent copper ion complexing agent as a leaching enhancer into a chalcopyrite biological leaching system, wherein the leaching enhancer reduces the chalcopyrite lattice stability by complexing with monovalent copper on the surface of the chalcopyrite, thereby promoting its oxidation leaching, and at the same time, synergistically regulating the potential and iron concentration of the leaching system, controlling the potential within a chalcopyrite leaching potential window of 580-650 mV (vs. SHE) and controlling the iron concentration within 2-5 g / L; through the synergistic effect of the three, chemical catalysis is enhanced, the oxidation of the chalcopyrite is promoted, the growth of acidophilic oxidizing microorganisms is beneficial, the activity of the microorganisms is ensured, the degradation rate of the leaching enhancer is reduced, the consumption thereof is reduced, the iron production is reduced, and the iron and acid discharge burdens of the system are reduced.
[0016] The leaching system refers to the combination of all substances involved in the leaching process.
[0017] Among them, the redox potential of the solution of the leaching system is controlled to be 580-650mV (vs.SHE), for example, it can be 580mV (vs.SHE), 590mV (vs.SHE), 600mV (vs.SHE), 610mV (vs.SHE), 620mV (vs.SHE), 630mV (vs.SHE), 640mV (vs.SHE) or 650mV (vs.SHE), but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] The iron concentration of the solution in the leaching system is controlled to be 2-5 g / L, for example, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or 5 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, the leaching enhancer comprises any one or a combination of at least two of acetylacetone, triphenylphosphine, tributylphosphine, nitromethane, dextran, hydroxyethylidene diphosphonic acid, ethyl acetoacetate, diester of malonate, imidazole, pyridine, methylthiourea, dimethylthiourea, tetramethylthiourea, n-propylthiourea, diisopropylthiourea, allylthiourea, ethylene trithiocarbonate, semicarbazide, phenylthiourea, tolylthiourea, chlorophenylthiourea, thiourea, ethylenethiourea, thioacetamide, dithizone, sodium dimethyldithiocarbamate or dithioformamidine, typical but non-limiting examples thereof. The combination includes a combination of acetylacetone and triphenylphosphine, a combination of tributylphosphine and nitromethane, a combination of dextran and hydroxyethylidene diphosphonic acid, a combination of malonic acid diester and pyridine, a combination of acetylacetone and methylthiourea, a combination of methylthiourea and dimethylthiourea, a combination of tetramethylthiourea and n-propylthiourea, a combination of diisopropylthiourea and allylthiourea, a combination of ethylene trithiocarbonate, semicarbazide and phenylthiourea, a combination of tolylthiourea, chlorophenylthiourea and thiourea, or a combination of ethylenethiourea, thioacetamide, sodium dimethyldithiocarbamate and dithioformamidine.
[0020] Preferably, the leaching enhancers are used in combination of at least two.
[0021] Preferably, the leaching enhancer is a combination of acetylacetone and imidazole, a combination of methylthiourea and dithizone, a combination of triphenylphosphine and dithiocarboxamidine, a combination of nitromethane and thiourea, or a combination of pyridine and ethylenethiourea.
[0022] The above-mentioned different types of copper ion complexing agents have different optimal conditions for action, such as pH, iron ion concentration, redox potential, etc. The combination of enhancers can adapt to the reaction conditions of different stages of chalcopyrite oxidation, achieve the enhancement of the entire leaching process, and further improve the copper leaching rate.
[0023] Preferably, the concentration of the leaching enhancer in the solution of the leaching system is 10-500 mg / L, for example, it can be 10 mg / L, 50 mg / L, 100 mg / L, 200 mg / L, 300 mg / L, 400 mg / L or 500 mg / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 50-200 mg / L.
[0024] Preferably, the redox potential is controlled by a potential regulator.
[0025] When the redox potential of the solution in the leaching system exceeds 650 mV, a potential regulator is added.
[0026] Preferably, the potential regulating agent includes any one of sodium sulfite, ascorbic acid, ammonium silicite, glycine, triethylenetetramine, sodium hexametaphosphate, sodium thiocyanate, sulfur dioxide, nitrite, iron powder or sodium sulfide, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium sulfite and ascorbic acid, a combination of ammonium silicite and glycine, a combination of triethylenetetramine and sodium hexametaphosphate, a combination of sodium thiocyanate and sulfur dioxide, or a combination of nitrite, iron powder and sodium sulfide.
[0027] Preferably, the iron concentration is controlled by adding alkali and / or heating.
[0028] When the iron concentration of the solution in the leaching system exceeds 5 g / L, iron removal is performed by adding alkali to precipitate iron ions and / or by heating to form iron alum compounds.
[0029] Preferably, the concentration of sulfuric acid in the microbial leaching extract is 2-10 g / L, for example, it can be 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L or 10 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] Preferably, the iron concentration in the microbial leaching extract is 2-5 g / L, for example, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or 5 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the leaching method comprises heap leaching and / or agitation leaching.
[0032] Preferably, the leaching temperature is 15-60°C, for example, 15°C, 20°C, 30°C, 40°C, 50°C or 60°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the acidophilic oxidizing microorganism comprises any one of Acidithiobacillus, Leptospirillum, Ferroplasma, Sulfobacillus or Sulfolobus, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of Acidithiobacillus and Leptospirillum, a combination of Ferroplasma and Sulfobacillus, a combination of Sulfobacillus and Sulfolobus, a combination of Acidithiobacillus, Leptospirillum and Acidithiobacillus, a combination of Ferroplasma, Sulfobacillus and Sulfolobus, or a combination of Acidithiobacillus, Leptospirillum, Ferroplasma, Sulfobacillus and Sulfolobus.
[0034] The acidophilic oxidizing microorganism is obtained from a patented preserved strain, acid mine wastewater or a biometallurgical production solution.
[0035] Preferably, the acidophilic oxidizing microorganism comprises any one or a combination of at least two of the acidophilic sulfur oxidizing microorganism Aciditiobacilluscaldus IPECAS, with a preservation number of CCTCC M 20221351, the acidophilic iron oxidizing microorganism Leptospirillumferriphilum ACID1, with a preservation number of CCTCC M 2013527, or the acidophilic iron oxidizing microorganism Leptospirillumferrooxidans ACID2, with a preservation number of CCTCC M 2013528.
[0036] The acidophilic sulfur-oxidizing microorganism Aciditiobacillus caldus IPECAS is classified and named Aciditiobacillus caldus, with a preservation number of CCTCC M 20221351, a preservation date of September 7, 2022, a preservation unit of the China Center for Type Culture Collection, and a preservation address of No. 299, Bayi Road, Wuchang District, Wuhan City, Hubei Province.
[0037] The acidophilic iron-oxidizing microorganism Leptospirillum ferriphilum ACID1 is classified and named Leptospirillum ferriphilum, with a preservation number of CCTCC M 2013527 and a preservation date of November 7, 2013. The preservation unit is China Center for Type Culture Collection, and the preservation address is No. 299, Bayi Road, Wuchang District, Wuhan City, Hubei Province.
[0038] The acidophilic iron-oxidizing microorganism Leptospirillum ferrooxidans ACID2 is classified and named Leptospirillum ferrooxidans, with a preservation number of CCTCC M 2013528 and a preservation date of November 7, 2013. The preservation unit is China Center for Type Culture Collection, and the preservation address is No. 299, Bayi Road, Wuchang District, Wuhan City, Hubei Province.
[0039] Preferably, the concentration of the acidophilic oxidizing microorganisms in the microbial leaching extract is 0.1×10 7 -10×10 7 cell / mL, for example, 0.1×10 7 cell / mL、0.5×10 7 cell / mL, 1×10 7 cell / mL, 2×10 7 cell / mL, 4×10 7 cell / mL、5×10 7 cell / mL、6×10 7 cell / mL、8×10 7 cell / mL or 10×10 7 cell / mL, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] Preferably, the method further comprises: extracting and electro-depositing the obtained leaching solution in sequence to obtain cathode copper.
[0041] By controlling the low iron concentration in the leaching process, the low iron concentration in the leaching solution is conducive to the selective extraction of copper. At the same time, less iron impurities enter the electrodeposition, and the electrodeposition efficiency is high.
[0042] Preferably, the raffinate obtained after the extraction is recycled for leaching.
[0043] Preferably, the P of the chalcopyrite ore 80 The particle size is 0.05-100 mm, for example, 0.05 mm, 0.1 mm, 1 mm, 10 mm, 30 mm, 50 mm, 80 mm or 100 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] Preferably, the chalcopyrite ore is an ore containing one or more sulfide minerals of chalcopyrite.
[0045] Preferably, the ore includes raw ore and / or enriched concentrate.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The method for enhancing biological leaching of chalcopyrite provided by the present invention uses a leaching enhancer and coordinates and regulates the leaching potential and the iron ion concentration, so as to realize efficient oxidation leaching of chalcopyrite, achieve a copper leaching rate of more than 82.8%, reduce the dissolution of non-copper sulfide minerals, reduce the acid and iron production during the leaching process, reduce the burden of iron removal and acid removal, improve the leaching efficiency of copper, and have low consumption of enhancing agents and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a process flow chart of the method provided in Example 1. DETAILED DESCRIPTION
[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0050] In order to clearly illustrate the technical solution of the present invention, the copper ore used in the examples is an ore whose main copper mineral is chalcopyrite, and the copper content is 0.45%.
[0051] Example 1
[0052] This embodiment provides a Figure 1 The method for enhanced bioleaching of chalcopyrite shown in the invention comprises the following steps:
[0053] (1) Crushing copper ore into P 80 The particle size was 20 mm. 10 mg / kg of methyl thiourea was added to the ore to enhance the leaching effect. Acidithiobacillus and Leptospirillum from acid mine wastewater were inoculated into the leaching extract with an iron concentration of 3 g / L and a sulfuric acid concentration of 5 g / L. The concentration of the microorganisms was 5×10 7 cell / mL, the leaching extract was added to the copper ore for heap leaching at 30°C for 180 days;
[0054] During the leaching process, methyl thiourea was added to maintain the concentration of methyl thiourea in the leaching extract at 100 mg / L, and the iron concentration in the leaching extract was controlled at 3 g / L. When the iron concentration in the extract increased, lime was added for neutralization and iron removal. At the same time, the potential of the extract was controlled at 600 mV (vs. SHE). When the potential increased, sodium sulfite was added;
[0055] (2) obtaining a leachate with a copper concentration higher than 4 g / L, extracting and enriching the copper ions in the leachate, and then performing electrodeposition to obtain cathode copper. The raffinate after extraction is further used for heap leaching. If the concentration of sulfuric acid in the raffinate is lower than 2 g / L, sulfuric acid is added thereto to a concentration of 5 g / L.
[0056] Example 2
[0057] This embodiment provides a method for enhanced bioleaching of chalcopyrite, the method comprising the following steps:
[0058] (1) Crushing copper ore into P 80 The particle size was 0.05 mm. 10 mg / kg of methyl thiourea, a leaching enhancer, was added to the ore. Acidithiobacillus and Leptospirillum from acid mine wastewater were inoculated into the leaching extract with an iron concentration of 2 g / L and a sulfuric acid concentration of 2 g / L. The concentration of the microorganisms was 0.1×10 7 cell / mL, the leaching extract was added to the copper ore and stirred and leached at 45°C for 20 days;
[0059] During the leaching process, methylthiourea was added to maintain the concentration of methylthiourea in the leaching extract at 10 mg / L, and the iron concentration in the leaching extract was controlled at 2 g / L. When the iron concentration in the extract increased, lime was added to remove iron. At the same time, the potential of the extract was controlled at 580 mV (vs. SHE). When the potential increased, sodium sulfite was added.
[0060] (2) obtaining a leachate with a copper concentration higher than 4 g / L, extracting and enriching the copper ions in the leachate, and then performing electrodeposition to obtain cathode copper. The raffinate after extraction is further used for stirring leaching. If the concentration of sulfuric acid in the raffinate is lower than 2 g / L, sulfuric acid is added thereto to a concentration of 5 g / L.
[0061] Example 3
[0062] This embodiment provides a method for enhanced bioleaching of chalcopyrite, the method comprising the following steps:
[0063] (1) Crushing copper ore into P 80 The particle size was 100 mm, 10 mg / kg of methyl thiourea was added to the ore, and the leaching extract with an iron concentration of 5 g / L and a sulfuric acid concentration of 10 g / L was inoculated with acidophilic thiobacillus and leptospirillum from acid mine wastewater. The concentration of the microorganisms was 10×10 7 cell / mL, the leaching extract was added to the copper ore for heap leaching at 60°C for 180 days;
[0064] During the leaching process, methylthiourea was added to maintain the concentration of methylthiourea in the leaching extract at 500 mg / L, and the iron concentration in the leaching extract was controlled at 5 g / L. When the iron concentration in the extract was higher than 5 g / L, lime was added to remove iron. At the same time, the potential of the extract was controlled at 650 mV (vs. SHE). When the potential increased, sodium sulfite was added.
[0065] (2) obtaining a leachate with a copper concentration higher than 4 g / L, extracting and enriching the copper ions in the leachate, and then performing electrodeposition to obtain cathode copper. The raffinate after extraction is further used for heap leaching. If the concentration of sulfuric acid in the raffinate is lower than 2 g / L, sulfuric acid is added thereto to a concentration of 5 g / L.
[0066] Example 4
[0067] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the concentration of methyl thiourea in step (2) is controlled to be 50 mg / L, and the rest is the same as Example 1.
[0068] Example 5
[0069] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the concentration of methylthiourea in step (2) is controlled to be 200 mg / L, and the rest is the same as Example 1.
[0070] Example 6
[0071] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the leaching enhancer is replaced with dimethylthiourea, and the rest is the same as Example 1.
[0072] Example 7
[0073] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the potential regulator is replaced by ascorbic acid, and the rest is the same as Example 1.
[0074] Example 8
[0075] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the inoculated acidophilic oxidizing microorganisms are replaced with equal concentrations of acidophilic sulfur-oxidizing microorganisms Aciditiobacillus caldus IPECAS, with a preservation number of CCTCC M 20221351, acidophilic iron-oxidizing microorganisms Leptospirillum ferriphilum ACID1, with a preservation number of CCTCC M 2013527, and Leptospirillum ferrooxidans ACID2, with a preservation number of CCTCC M2013528. The rest are the same as in Example 1.
[0076] Example 9
[0077] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the 10 mg / kg methyl thiourea enhancer added to the ore is replaced by 10 mg / kg methyl thiourea and dithizone in total, and the sum of the concentrations of the two is maintained at 100 mg / L during the leaching process. The rest is the same as Example 1.
[0078] Example 10
[0079] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the enhanced agent methyl thiourea 10 mg / kg added to the ore is replaced by 10 mg / kg of acetylacetone and imidazole, and the sum of the concentrations of the two is maintained at 100 mg / L during the leaching process. The rest is the same as Example 1.
[0080] Embodiment 11
[0081] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the enhanced agent methyl thiourea 10 mg / kg added to the ore is replaced by triphenylphosphine and disulfide formamidine 10 mg / kg in total, and the sum of the concentrations of the two is maintained at 100 mg / L during the leaching process. The rest is the same as Example 1.
[0082] Example 12
[0083] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the enhanced agent methylthiourea 10 mg / kg added to the ore is replaced by nitromethane and thiourea 10 mg / kg in total, and the sum of the concentrations of the two is maintained at 100 mg / L during the leaching process. The rest is the same as Example 1.
[0084] Example 13
[0085] This embodiment provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, the enhanced agent methyl thiourea 10 mg / kg added to the ore is replaced by pyridine and ethylene thiourea 10 mg / kg in total, and the sum of the concentrations of the two is maintained at 100 mg / L during the leaching process. The rest is the same as Example 1.
[0086] Comparative Example 1
[0087] This comparative example provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, no leaching enhancer is added during the leaching process, and the rest is the same as Example 1.
[0088] Comparative Example 2
[0089] This comparative example provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, no potential regulator is added during the leaching process, and the rest is the same as Example 1.
[0090] In this comparative example, during the leaching process, the redox potential of the solution of the leaching system reached 850 mV (vs. SHE).
[0091] Comparative Example 3
[0092] This comparative example provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, no iron removal is performed during the leaching process, and the rest is the same as Example 1.
[0093] In this comparative example, during the leaching process, the iron concentration of the solution in the leaching system reached 45 g / L.
[0094] Comparative Example 4
[0095] This comparative example provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, no leaching enhancer and potential regulator are added during the leaching process, and the rest is the same as Example 1.
[0096] In this comparative example, during the leaching process, the redox potential of the solution of the leaching system reached 842 mV (vs. SHE).
[0097] Comparative Example 5
[0098] This comparative example provides a method for enhanced bioleaching of chalcopyrite. Compared with Example 1, no leaching enhancer and potential regulator are added, and iron removal is not performed. The rest is the same as Example 1.
[0099] In this comparative example, during the leaching process, the redox potential of the solution of the leaching system reached 796 mV (vs. SHE), and the iron concentration reached 38.5 g / L.
[0100] Table 1
[0101] Copper leaching rate (%) Leaching enhancer consumption (kg / t) Example 1 82.8 0.75 Example 2 89.6 1.25 Example 3 87.6 2.58 Example 4 85.2 1.24 Example 5 92.5 2.02 Example 6 83.5 0.74 Example 7 84.3 0.76 Example 8 92.5 0.78 Example 9 88.5 0.64 Example 10 89.3 0.61 Embodiment 11 90.2 0.53 Example 12 90.5 0.46 Example 13 90.6 0.52 Comparative Example 1 35.2 0 Comparative Example 2 62.8 4.25 Comparative Example 3 70.3 3.86 Comparative Example 4 30.1 0 Comparative Example 5 21.2 0
[0102] Performance Testing
[0103] The enhanced bioleaching process of chalcopyrite was simulated in a shaking table, and a comparative test of leaching conditions was carried out.
[0104] In a shaker, copper ore crushed to a P80 particle size of 0.05 mm, microbial leaching extract and leaching enhancer thiourea were added, with a thiourea concentration of 100 mg / L and an Acidithiobacillus concentration of 5 × 10 7 cell / mL, under the conditions of sulfuric acid concentration of 5g / L, iron concentration of 5g / L, and 30℃, the solution potential in the shaking table was controlled at 550mV (vs.SHE), 650mV (vs.SHE), 750mV (vs.SHE) and 850mV (vs.SHE), respectively, and the reaction was carried out for 10 days respectively. The leaching rate of copper and the degradation rate of the leaching enhancer were determined. The results are shown in Table 2.
[0105] Table 2
[0106] Solution potential (mV, vs. SHE) Copper leaching rate (%) Degradation rate of leaching enhancer (%) 550 42.5 4.1 650 88.6 3.5 750 30.6 36.2 850 40.2 42.5
[0107] In a shaker, add crushed 80 Copper ore with a particle size of 0.05 mm, microbial leaching extract, and Acidithiobacillus concentration of 5×10 7 cell / mL, different leaching enhancers were added respectively, and the leaching enhancers selected were thiourea, disulfide formamidine, triphenylphosphine, ethylene thiourea and thioacetamide. Under the conditions of sulfuric acid concentration of 5g / L, iron concentration of 5g / L, and 30℃, the reaction was carried out for 10 days respectively. During the leaching process, the potential of the solution was controlled at 650mV (vs.SHE), and the leaching rate of copper and the degradation rate of the leaching enhancer were determined. The results are shown in Table 3.
[0108] Table 3
[0109]
[0110]
[0111] It can be seen from the data in Tables 1-3 that the enhanced bioleaching method provided by the present invention can effectively leach chalcopyrite, the leaching rate of copper can reach more than 82.8%, and the reduction rate and consumption of the enhanced leaching agent are low.
[0112] The method provided by the present invention realizes efficient leaching of chalcopyrite by synergistic coupling of chemical enhanced leaching, potential regulation and iron concentration control. The main technical effects and reasons include: (1) high microbial activity: low iron content and low potential are conducive to the growth of acidophilic iron-sulfur oxidizing bacteria; (2) reduced consumption of enhanced leaching reagents: under low iron concentration and low potential conditions, the degradation rate of the reagents is significantly reduced; (3) reduced iron removal: under low potential conditions, pyrite oxidation is reduced or even stagnant, and the iron production is significantly reduced; (4) high chalcopyrite oxidation rate: through stable chemical catalytic enhancement, the chalcopyrite leaching potential window is met and high microbial activity is maintained; (5) high extraction-electrodeposition efficiency: low iron concentration is conducive to the selective extraction of copper, and at the same time, less iron impurities enter the electrodeposition, and the electrodeposition efficiency is high.
[0113] In summary, the method for enhanced bioleaching of chalcopyrite provided by the present invention uses a leaching enhancer and coordinates and regulates the leaching potential and the iron ion concentration to achieve efficient oxidation leaching of chalcopyrite, the copper leaching rate reaches more than 82.8%, the dissolution of non-copper sulfide minerals is reduced, the acid and iron production during the leaching process is reduced, the burden of iron removal and acid removal is reduced, the leaching efficiency of copper is improved, and the consumption of the enhancing agent is low and the cost is low.
[0114] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for enhanced bioleaching of chalcopyrite, characterized in that: The method comprises: The chalcopyrite ore, the microbial leaching extract and the leaching enhancer are mixed and leached to obtain a leaching solution; The microbial leaching extract is an acidic ferric iron solution containing acidophilic oxidizing microorganisms; During the leaching process, the redox potential of the solution of the leaching system is controlled to be 580-650 mV (vs. SHE), and the iron concentration in the solution is controlled to be 2-5 g / L.
2. The method according to claim 1, characterized in that The leaching enhancer comprises any one of acetylacetone, triphenylphosphine, tributylphosphine, nitromethane, diglucan, hydroxyethylidene diphosphonic acid, ethyl acetoacetate, diester of malonate, imidazole, pyridine, methylthiourea, dimethylthiourea, tetramethylthiourea, n-propylthiourea, diisopropylthiourea, allylthiourea, ethylene trithiocarbonate, semicarbazide, phenylthiourea, tolylthiourea, chlorophenylthiourea, thiourea, ethylenethiourea, thioacetamide, dithizone, sodium dimethyldithiocarbamate or dithioformamidine, or a combination of at least two thereof; Preferably, the leaching enhancer uses a combination of at least two; Preferably, the leaching enhancer is a combination of acetylacetone and imidazole, a combination of methylthiourea and dithizone, a combination of triphenylphosphine and dithiocarboxamidine, a combination of nitromethane and thiourea, or a combination of pyridine and ethylenethiourea.
3. The method according to claim 1 or 2, characterized in that: The concentration of the leaching enhancer in the solution of the leaching system is 10-500 mg / L, preferably 50-200 mg / L.
4. The method according to any one of claims 1 to 3, characterized in that: The redox potential is controlled by a potential regulator; Preferably, the potential regulator includes any one or a combination of at least two of sodium sulfite, ascorbic acid, ammonium silicite, glycine, triethylenetetramine, sodium hexametaphosphate, sodium thiocyanate, sulfur dioxide, nitrite, iron powder or sodium sulfide.
5. The method according to any one of claims 1 to 4, characterized in that: The iron concentration is controlled by adding alkali and / or heating.
6. The method according to any one of claims 1 to 5, characterized in that: The concentration of sulfuric acid in the microbial leaching extract is 2-10 g / L; Preferably, the concentration of iron in the microbial leaching extract is 2-5 g / L.
7. The method according to any one of claims 1 to 6, characterized in that: The leaching method includes heap leaching and / or agitation leaching; Preferably, the leaching temperature is 15-60°C.
8. The method according to any one of claims 1 to 7, characterized in that: The acidophilic oxidizing microorganisms include any one or a combination of at least two of Acidithiobacillus, Leptospirillum, Ferrobacterium, Sulfobacillus or Sulfolobus; Preferably, the concentration of the acidophilic oxidizing microorganisms in the microbial leaching extract is 0.1×10 7 -10×10 7 cell / mL.
9. The method according to any one of claims 1 to 8, characterized in that: The method further comprises: extracting and electro-depositing the obtained leaching solution in sequence to obtain cathode copper; Preferably, the raffinate obtained after the extraction is recycled for leaching.
10. The method according to any one of claims 1 to 9, characterized in that: The P of the chalcopyrite ore 80 Particle size is 0.05-100mm; Preferably, the chalcopyrite ore is an ore containing one or more sulfide minerals of chalcopyrite; Preferably, the ore includes raw ore and / or enriched concentrate.
Citation Information
Patent Citations
Method of promoting bioleaching of copper pyrites by adding nonionic surfactant
CN103993171A
Method for reinforcing leaching of chalcopyrite microorganisms
CN105861823A
Process for leaching metal sulfides with reagents having thiocarbonyl functional groups
CN110352256A
Method for enhancing bioleaching of chalcopyrite through flotation collecting agent
CN115287453A
Leaching copper-containing ores
CN111194358A
Cited By
Chalcopyrite bioleaching method based on synergistic effect of mechanical activation and potential regulation
CN120249679A