Nickel-silicon-copper alloy electroslag production process
By using a pre-melted slag system of CaF2:MgF2=90:10, graphite electrode arc initiation, and argon protection, the electroslag remelting process for nickel-silicon-copper alloys solved the problems of slag channels and slag wrapping at the ingot tail caused by the low melting point of nickel-silicon-copper alloys, and achieved high-quality nickel-silicon-copper alloy production.
Patent Information
- Application Number
- CN202410803837.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-08
AI Technical Summary
The low melting point of existing nickel-silicon-copper alloys makes it difficult to match the slag system during electroslag remelting, which easily leads to defects such as slag grooves and slag wrapping at the ingot tail. Furthermore, traditional casting methods cannot guarantee the quality stability and purity of the alloy.
A pre-melted slag system of CaF2:MgF2=90:10 was used. Graphite electrodes were used for arc initiation and argon protection. The melting rate and power supply parameters were controlled. Calcium silicon powder was added for deoxidation, and the water temperature difference was controlled to ensure the smelting quality of the alloy.
It improves the corrosion resistance and ductility of nickel-silicon-copper alloys, solves the problem of slag entrapment in slag channels and ingot tails, and ensures the internal quality and surface smoothness of the alloy.
Smart Images

Figure CN118910415A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electroslag metallurgy, and relates to an electroslag production process for a nickel-silicon-copper alloy used for manufacturing marine vessels and having excellent corrosion resistance and ductility. The present invention can effectively solve the problem that the corresponding melting point will be reduced during the production process of the nickel-silicon-copper alloy, resulting in difficulty in slag system matching in the electroslag process. Technical Background
[0002] The nickel-silicon-copper alloy has a copper content of more than 90%, has the characteristics of ultra-low resistance, high hardness and corrosion resistance, and is a good material for marine ships. At present, this type of alloy on the market is mainly produced by continuous casting or oxidation protection casting. Continuous casting is to continuously pour the molten alloy into cooling water to make alloy billets, which has the characteristics of high efficiency and energy saving. Oxidation protection casting is to introduce a gas-oxygen mixture into the furnace body to control the redox reaction and prevent the alloy from being oxidized and polluted by air. Although the two casting methods can guarantee the purity of the billet to a certain extent, their quality stability is insufficient, and the nickel-silicon-copper alloy billet produced by them is prone to looseness and high inclusion levels. Electroslag remelting can effectively improve the above problems. The resistance heat generated when the current passes through the slag is used as a heat source to re-smelt the nickel-silicon-copper alloy, improve the crystallization of the alloy casting, and make its structure denser and more uniform in composition. However, since the composition design requirements of nickel-silicon-copper alloy are: Cu: 93-98%, Ni: 2-4%, Si≤1%, Cr≤1%, Fe≤0.005%, the nickel-silicon-copper alloy has a very large Cu content, resulting in a low melting point of only about 1050°C. The two- to three-component slag system based on CaF2, Al2O3, and CaO commonly used in the field of electroslag has a melting point of about 1300-1400°C, which is higher than the melting point of the nickel-silicon-copper alloy itself, making it easy to produce slag grooves on the surface during smelting. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a nickel-silicon-copper alloy electroslag production process that replaces the traditional casting production process and produces finished products with better quality and higher stability.
[0004] The technical solution of the present invention is achieved as follows: a nickel-silicon-copper alloy electroslag production process, wherein the nickel-silicon-copper alloy comprises, by mass percentage, Cu: 93-98%, Ni: 2-4%, Si≤1%, Cr≤1%, and Fe≤0.005%; the specific process steps are as follows:
[0005] Step 1), configure the electroslag slag system for nickel-silicon-copper alloy electroslag production: the electroslag slag system selected is a pre-melted slag of CaF2:MgF2=90:10 according to the mass ratio and state;
[0006] Step 2), arcing, slag removal and gas protection: Graphite electrodes are used for arc starting, argon gas is used for protection during the production process, and asbestos is used to block the furnace body from the outside world;
[0007] Step 3), control the melting rate: the melting rate is controlled at 0.75 to 1.2 times the diameter of the crystallizer, and the internal control target average melting rate is 470 kg / h;
[0008] Step 4) Control power supply parameters: The current and voltage of the electroslag process are controlled to be stable, and the current fluctuation is controlled to be ≤±15%:
[0009] Step 5), control the deoxidation system: use calcium silicon powder for deoxidation, add 270-300g calcium silicon powder for every 100kg nickel-silicon-copper alloy for deoxidation; adopt staged addition, add 110-120g calcium silicon powder every 5 minutes at the beginning of current increase, and change to add 50-60g calcium silicon powder every 5 minutes after the shrinkage feeding stage;
[0010] Step 6) Water temperature control: During the remelting process, the total inlet water temperature is controlled, and the temperature difference between the inlet and outlet water of the crystallizer is controlled to be ≤15°C.
[0011] The present invention has the following positive effects:
[0012] The nickel-silicon-copper alloy is used for making marine vessels, and it needs to have excellent corrosion resistance and ductility, so its composition range is designed to be: Cu: 93-98%, Ni: 2-4%, Si≤1%, Cr≤1%, Fe≤0.005%. The nickel-silicon-copper alloy has a low melting point of only about 1050°C due to its extremely high Cu content. The melting point of the two- to three-component slag system based on CaF2, Al2O3, and CaO commonly used in the field of electroslag is about 1300-1400°C, which is higher than the melting point of the nickel-silicon-copper alloy itself, making it easy to produce slag grooves on the surface during smelting. Therefore, the slag system of nickel-silicon-copper alloy electroslag cannot use the 73 slag system and 65:25:10 slag system commonly used in the field of electroslag, but other components should be used for proportioning to reduce the melting point of the slag system.
[0013] The arc starting method in the production of nickel-silicon-copper alloy electroslag is to use a graphite electrode for arc starting, and the nickel-silicon-copper alloy body cannot be used for arc starting. The melting point of this steel is extremely low, and when the body is used for arc starting, it is easy for the body to melt before the slag, resulting in slag wrapping defects at the ingot tail.
[0014] During the nickel-silicon-copper alloy electroslag production, the melting rate is set internally to 1.0 times the crystallizer diameter. When the set melting rate exceeds 1.2 times the crystallizer diameter, it will cause loose defects at the tail end of the nickel-silicon-copper electroslag ingot. When the set melting rate is less than 0.75 times the crystallizer diameter, the ingot surface forming quality is poor.
[0015] The nickel-silicon-copper alloy electroslag is produced under argon protection and with the addition of calcium silicon powder, which blocks the furnace from the outside world, preventing the electroslag ingot from increasing O and preventing the nickel-silicon-copper alloy from oxidizing when it is heated and melted and in contact with the atmosphere.
[0016] The present invention relates to a nickel-silicon-copper alloy electroslag remelting process, wherein the nickel-silicon-copper alloy needs to have excellent corrosion resistance and thermal conductivity, and its composition range is designed to be: Cu: 93-98%, Ni: 2-4%, Si≤1%, Cr≤1%, Fe≤0.005%. The melting point of the nickel-silicon-copper alloy is only 1050°C, which is extremely low. The traditional two- to three-component slag system based on CaF2, Al2O3, and CaO cannot be used. Components that can reduce the melting point must be added for production to prevent the steel slag from combining and forming slag grooves during production. The nickel-silicon-copper alloy needs to use a graphite electrode for arc starting to prevent the copper alloy body from melting first when slagging, resulting in slag wrapping defects at the bottom. The melting speed of the nickel-silicon-copper alloy electroslag is set to be 1.0 times the diameter of the crystallizer during production to prevent looseness or poor surface molding quality. Argon protection is used for production and a deoxidizer is added to control the oxygen content. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic diagram showing that the 1# bottom pores on the surface of the electroslag ingot after the mold is lifted according to the present invention are serious.
[0018] Figure 2 It is a schematic diagram of the 2# through-body slag groove on the surface of the electroslag ingot after the mold is lifted according to the present invention.
[0019] Figure 3 This is a schematic diagram showing that the surface of the 3# electroslag ingot is smooth and has no pores after the mold is lifted, and the internal quality is flat after sawing. DETAILED DESCRIPTION
[0020] The present invention relates to a nickel-silicon-copper alloy electroslag remelting process. The nickel-silicon-copper alloy needs to have excellent corrosion resistance and ductility, and its composition range is designed to be: Cu: 93-98%, Ni: 2-4%, Si≤1%, Cr≤1%, Fe≤0.005%. The melting point of the nickel-silicon-copper alloy is only 1050°C, which is extremely low. The traditional two- to three-component slag system based on CaF2, Al2O3, and CaO cannot be used to prevent the steel slag from combining and forming slag grooves during production. The nickel-silicon-copper alloy needs to use a graphite electrode for arc starting. During the production of the nickel-silicon-copper alloy electroslag, the melting speed is set to 1.0 times the diameter of the crystallizer, and argon protection is used for production and a deoxidizer is added. The specific implementation plan is as follows:
[0021] A nickel-silicon-copper alloy electroslag production process, wherein the nickel-silicon-copper alloy comprises, by mass percentage, Cu: 93-98%, Ni: 2-4%, Si≤1%, Cr≤1%, Fe≤0.005%; the specific process steps are as follows:
[0022] Step 1), configure the electroslag slag system for nickel-silicon-copper alloy electroslag production: the electroslag slag system selected is a pre-melted slag of CaF2:MgF2=90:10 according to the mass ratio and state;
[0023] Step 2), arcing, slag removal and gas protection: Graphite electrodes are used for arc starting, argon gas is used for protection during the production process, and asbestos is used to block the furnace body from the outside world;
[0024] Step 3), control the melting rate: the melting rate is controlled at 0.75 to 1.2 times the diameter of the crystallizer, and the internal control target average melting rate is 470 kg / h;
[0025] Step 4) Control power supply parameters: The current and voltage of the electroslag process are controlled to be stable, and the current fluctuation is controlled to be ≤±15%:
[0026] Step 5), control the deoxidation system: use calcium silicon powder for deoxidation, add 270-300g calcium silicon powder for every 100kg nickel-silicon-copper alloy for deoxidation; adopt staged addition, add 110-120g calcium silicon powder every 5 minutes at the beginning of current increase, and change to add 50-60g calcium silicon powder every 5 minutes after the shrinkage feeding stage;
[0027] Step 6) Water temperature control: During the remelting process, the total inlet water temperature is controlled, and the temperature difference between the inlet and outlet water of the crystallizer is controlled to be ≤15°C.
[0028] Comparative Example 1:
[0029] 1. Production details:
[0030]
[0031] 2. CaF2 is used in combination with MgF2 and CaO for the 1# slag material of nickel-silicon-copper electroslag ingot. MgF2 is used to replace Al2O3 to reduce the melting point of the slag. CaF2 is used in combination with MgF2 and BaCl2 for the 2# slag material of nickel-silicon-copper electroslag ingot. BaCl2 is added to increase the ion concentration in the slag, thereby improving the conductivity of the slag system.
[0032] Slag system 1: CaF2: MgF2: CaO = 60: 20: 20
[0033] Slag system 2: CaF2: MgF2: BaCl2 = 60: 20: 20
[0034] Slag volume: 20kg
[0035] 3. Arcing, slag removal and gas protection:
[0036] Graphite electrodes are used to start the arc and argon gas is used for protection during the production process.
[0037] 4. Melting rate:
[0038] The internal control target average melting rate is 270kg / h.
[0039] 5. Power supply system:
[0040]
[0041]
[0042] 6. Deoxygenation system:
[0043] Add calcium silicate powder for deoxidation, start to add calcium silicate powder at 60-70g / 5 minutes when the current is increased, and add 30-40g / 5 minutes during the shrinkage compensation stage.
[0044] 7. Quality of electroslag ingot:
[0045] After the mold was lifted, the surface of the electroslag ingot was observed and it was found that the bottom of the electroslag ingot 1# was seriously porous and the slag grooves were all over the body of the electroslag ingot 2#. Figure 1 , 2 shown.
[0046] Through analysis, it is known that the magnesium fluoride slag has a high content of crystal water, which cannot be completely removed during the slag baking stage. In addition, CaO is very easy to absorb moisture, which causes pores to appear at the bottom of the copper ingot during production. The excessive addition of BaCl2 causes the overall viscosity of the slag system to change, which affects the smelting and produces slag grooves.
[0047] Summarizing the defects of 1# and 2# copper ingots, the present invention adopts slag system 3 (CaF2:MgF2=90:10) for production.
[0048] Embodiment 1:
[0049] 1. Production details:
[0050]
[0051] 2. Nickel-silicon-copper 3# slag material is made of CaF2 and MgF2, and CaF2 and MgF2 are pre-melted before production to form pre-melted slag before use.
[0052] Slag system 3: 91 pre-melted slag (CaF2:MgF2=90:10)
[0053] Slag volume: 70kg
[0054] 3. Arcing, slag removal and gas protection:
[0055] Graphite electrodes are used to start the arc and argon gas is used for protection during the production process.
[0056] 4. Internal control target average melting rate 470kg / h.
[0057] 5. Power supply system:
[0058]
[0059] 6. Deoxygenation system:
[0060] Add calcium silicate powder for deoxidation, start to add calcium silicate powder at 110-120g / 5 minutes when the current is increased, and add 50-60g / 5 minutes during the shrinkage compensation stage.
[0061] 7. Water temperature control:
[0062] During the remelting process, the total inlet water temperature is controlled, and the temperature difference between the inlet and outlet water of the crystallizer is controlled to be ≤15℃.
[0063] 8. Quality of electroslag ingot:
[0064] After the mold is lifted, the surface of the electroslag ingot is observed. The surface of the 3# electroslag ingot is smooth and has no pores. The internal quality is flat after sawing. Figure 3 shown.
[0065] The trial production results show that the nickel-silicon-copper alloy electroslag ingot produced by the slag system 3 (CaF2:MgF2=90:10 and pre-melted) of the present invention has excellent product quality, smooth ingot surface and no internal defects. The nickel-silicon-copper alloy electroslag production has been successfully realized.
Claims
1. A nickel-silicon-copper alloy electroslag production process, characterized in that: The nickel-silicon-copper alloy has the following components according to mass percentage: Including: Cu: 93~98%, Ni: 2~4%, Si≤1%, Cr≤1%, Fe≤0.005%; the specific process steps are as follows: Step 1), configure the electroslag slag system for nickel-silicon-copper alloy electroslag production: the electroslag slag system selected is a pre-melted slag of CaF2:MgF2=90:10 according to the mass ratio and state; Step 2), arcing, slag removal and gas protection: Graphite electrodes are used for arc starting, argon gas is used for protection during the production process, and asbestos is used to block the furnace body from the outside world; Step 3), control the melting rate: the melting rate is controlled at 0.75~1.2 times the diameter of the crystallizer, and the internal control target average melting rate is 470kg / h; Step 4) Control power supply parameters: The current and voltage of the electroslag process are controlled to be stable, and the current fluctuation is controlled to be ≤±15%: Step 5), control the deoxidation system: use calcium silicon powder for deoxidation, add 270-300g calcium silicon powder for every 100kg nickel-silicon-copper alloy for deoxidation; adopt staged addition, add 110-120g calcium silicon powder every 5 minutes at the beginning of current increase, and change to add 50-60g calcium silicon powder every 5 minutes after the shrinkage feeding stage; Step 6) Water temperature control: Control the total inlet water temperature during the remelting process, and control the temperature difference between the inlet and outlet water of the crystallizer to ≤15℃.