Complex copper resource short-process smelting method

By smelting complex copper resources and multi-source cold materials under oxygen-rich conditions in copper smelting, and combining blow-refining and reducing vulcanization processes, efficient smelting of copper smelting and recycling of valuable metals is achieved, solving the problem of The problems of low copper smelting efficiency and environmental pollution in the existing technology have been promoted to innovation in copper smelting technology.

CN118910421APending Publication Date: 2024-11-08CENT SOUTH UNIV +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410931917.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing copper smelting process has problems such as low production efficiency, high environmental pollution, and the inability to effectively deal with complex copper resources and multi-source cold materials. The high-quality copper concentrate resources are depleted, so it is necessary to develop new copper resources with strong adaptability and high smelting strength. Process method.

Method used

Complex copper resources, fluxes, and multi-source cold materials are used to smelify under oxygen-rich conditions, and then smel them in a blow-refining furnace. Combined with the reduction vulcanization process, valuable metals are recovered, and copper smel is blown and smelted by optimizing the process flow. Coarse copper refining is coupled in one furnace, shortening the process and reducing costs.

Benefits of technology

The short process smelting of copper resources with strong raw materials adaptability, short process, high smelting efficiency, low flue gas and high copper direct yield has been achieved, which has improved production efficiency, reduced environmental pollution, and promoted the innovation of copper smelting technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910421A_ABST
    Figure CN118910421A_ABST
Patent Text Reader

Abstract

A short-process smelting method for complex copper resources comprises the following steps that (1) the complex copper resources, flux and multi-source cold charge are mixed, matte smelting is conducted under the oxygen-enriched condition, and high-grade copper matte, smelting slag and flue gas are obtained; (2) the high-grade copper matte is matched with a flux and then smelted in a blowing-refining furnace, and blowing slag, anode copper and flue gas are obtained; and (3) the smelting slag obtained in the step (1) is cooperatively matched with a vulcanizing agent and a reducing agent, copper matte, depleted slag and flue gas are obtained after reduction vulcanization, and valuable metal such as lead and zinc is recycled from the flue gas. According to the method, complex copper resources and multi-source cold materials are cooperatively matched, so that the bottleneck problem that an existing copper smelting technology cannot be adapted is solved; guidance is provided for efficient cleaning treatment of complex copper resources and comprehensive recovery of valuable multi-metal; the copper matte blowing process and the crude copper refining process are coupled in one furnace, qualified anode copper is directly produced for anode plate casting, the process is shortened, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical engineering, and in particular relates to a short-process smelting method for complex copper resources. Background Art

[0002] Copper is an important industrial raw material and strategic material, widely used in electrical, construction, machinery manufacturing, national defense and military industries.

[0003] Pyrometallurgy is the main process for producing metallic copper. Copper concentrate undergoes the processes of "matte smelting → matte blowing → crude copper refining" to produce anode copper. In the conventional copper smelting process, the above processes are completed intermittently in multiple furnaces, and the intermediate products of smelting need to be transported in multiple workshops by crane, which leads to problems such as low production efficiency and severe environmental pollution. With the depletion of high-quality copper concentrate resources, complex primary resources and secondary resources have become the main processing objects, and the global awareness of environmental protection continues to increase. It is urgent to develop a new continuous copper smelting method with strong raw material adaptability, high smelting intensity and large processing capacity. Efficient utilization of copper resources and innovation of environmentally friendly smelting technology are the key to meeting the current dual challenges of resource shortage and environmental protection. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a short-process smelting method for complex copper resources with strong raw material adaptability, shorter process, higher smelting efficiency, less flue gas and higher direct copper recovery rate.

[0005] The technical solution adopted by the present invention to solve the technical problem is a short-process smelting method for complex copper resources, comprising the following steps:

[0006] (1) Mixing complex copper resources with flux and multi-source cold materials, and smelting them under oxygen-rich conditions to obtain high-grade copper matte, smelting slag and flue gas;

[0007] (2) the high-grade copper matte is mixed with flux and smelted in a blowing-refining furnace to obtain blowing slag, anode copper and flue gas;

[0008] The blown slag can be returned to the matte smelting process in step (1) as multi-source cold material;

[0009] (3) The smelting slag obtained in step (1) is combined with a sulfiding agent and a reducing agent to perform reduction sulfidation to obtain copper matte, depleted slag and flue gas, and valuable metals such as lead and zinc are recovered from the flue gas;

[0010] The copper matte can be returned to the matte making and smelting process in step (1) as multi-source cold material.

[0011] In the above-mentioned short-process smelting method, preferably, in step (1), the complex copper resources include, in terms of mass percentage, 19-30% Cu, 22-28% Fe, 20-30% S, 0.5-1.0% Pb, and 1.5-2.45% Zn.

[0012] In the above short-process smelting method, preferably, in step (1), the flux is quartz sand, and the addition amount is 4-8% of the mass of the complex copper resource. In the matte smelting process, the iron-silicon slag type is used, and quartz sand needs to be added to ensure a suitable iron-silicon mass ratio. The iron-silicon mass ratio is controlled at 1.6-2.0, and a low melting point slag type can be obtained, thereby reducing energy consumption.

[0013] In the above short-process smelting method, preferably, in step (1), the multi-source cold material is one or more of low-grade copper ore (Cu mass percentage <15%), waste circuit boards, copper-containing sludge, waste copper, residual electrode cold material, etc., and the added amount is 5-10% of the mass of the complex copper resources. Matte smelting is an autothermal process. The addition of multi-source cold materials can reduce the smelting temperature and reduce the erosion of the slag on the furnace lining on the one hand, and can comprehensively recover the valuable metals in the multi-source cold materials on the other hand.

[0014] In the above short-process smelting method, preferably, in step (1), oxygen is blown into the furnace under the oxygen-enriched condition, and the blowing rate of oxygen is 10000-30000Nm 3 / h, oxygen enrichment concentration is 70-82%, oxygen-ore ratio is 145-165Nm 3 / t. The main reactions of blowing in oxygen are as follows:

[0015] CuFeS2+2.5O2=Cu2S·FeS+FeO+2SO2 (1)

[0016] 2FeS+3O2=2FeO+2SO2 (2)

[0017] 2Cu2S+3O2=2Cu2O+2SO2 (3)

[0018] FeS+Cu2O=FeO+Cu2S (4)

[0019] FeO+SiO2=FeO·SiO2 (5)

[0020] In the above short-process smelting method, preferably, in step (1), the smelting temperature is 1180-1250° C. and the smelting time is 0.5-2 hours.

[0021] In the above short-process smelting method, preferably, in step (1), the high-grade copper matte includes 73-78% Cu and 16-21% S in terms of mass percentage; the smelting slag includes 3-5% Cu, 0.3-1.0% Pb (lead), and 1.5-4.0 Zn. The matte smelting is carried out in a strong oxidizing atmosphere, resulting in a high copper content in the slag. The reduction sulfidation process can be used to recover valuable metals such as copper, lead, and zinc in the copper smelting slag.

[0022] In the above short-process smelting method, preferably, in step (2), the flux is quartz sand, and the added amount is equivalent to 5-12% of the mass of the high-grade copper matte.

[0023] In the above short-process smelting method, preferably, in step (2), a mixed gas is introduced into the blowing-refining furnace, and the smelting in the blowing-refining furnace includes two processes, an oxidation period and a reduction period. The pure oxygen injection rate during the oxidation period is 2000-2500Nm 3 / h, air blowing rate is 14000-16000Nm 3 / h, nitrogen injection rate is 5000-6000Nm 3 / h, the reaction time is 12-16h; the pure oxygen injection rate during the reduction period is 20-30Nm 3 / h, air blowing rate is 1000-1600Nm 3 / h, natural gas injection rate is 250-450Nm 3 / h, reaction time is 2-4h.

[0024] The pure oxygen refers to oxygen with a purity greater than or equal to 99.99%.

[0025] The present invention couples the copper matte blowing and blister copper refining processes in one furnace, completes the copper matte blowing and blister copper refining processes in one furnace by precisely controlling the gas blowing, and directly produces qualified anode copper for anode plate casting.

[0026] In the above short-process smelting method, preferably, in step (2), the blowing and refining temperature is 1220-1270°C.

[0027] In the above short-process smelting method, preferably, in step (2), the anode copper comprises 99.01-99.55% Cu (with a purity of 99.01-99.55%) in terms of mass percentage. The blowing slag can be returned to the matte smelting process in step (1). The direct copper recovery rate of the whole process is greater than 95%.

[0028] In the above short-process smelting method, preferably, in step (3), the sulfiding agent is one or more of sulfur, pyrite, calcium sulfate and gypsum slag, and the added amount is 2-15% of the mass of the smelting slag. The sulfiding agent is added mainly to provide a sulfur source for the depletion of the smelting slag and sulfidize Cu2O into Cu2S; when the amount of the sulfiding agent added is excessive, the Zn element in the slag will be converted into ZnS, reducing the zinc recovery rate.

[0029] In the above short-process smelting method, preferably, in step (3), the reducing agent is one or more of coke, anthracite, bituminous coal and biochar, and the amount added is 4-8% of the mass of the smelting slag. Copper smelting slag contains a large amount of high-melting-point Fe3O4, and the addition of the reducing agent reduces the high-valent iron oxide to FeO to form slag; if the amount of reducing agent added is too much, the iron oxide will be reduced to elemental iron, which will deteriorate the properties of the slag.

[0030] In the above short-process smelting method, preferably, in step (3), the reduction sulfidation temperature is 1200-1350°C, and the constant temperature time is 2-5h.

[0031] In the above-mentioned short-process smelting method, preferably, in step (3), valuable metals such as lead and zinc are recovered from the flue gas, wherein the lead recovery rate is greater than 98%, and the zinc recovery rate is greater than 85%.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention innovatively combines complex copper resources with multi-source cold materials to meet the fluctuation of copper resource raw materials in my country, solves the bottleneck problem that existing copper smelting technology cannot adapt to; determines the optimized process conditions and control measures, and provides guidance for the efficient and clean treatment of complex copper resources and the comprehensive recovery of valuable multi-metals;

[0034] (2) The present invention innovatively couples the copper matte blowing and crude copper refining processes in one furnace, directly producing qualified anode copper for anode plate casting, shortening the process and reducing costs;

[0035] (3) The present invention innovatively adopts a reduction sulfidation process for copper smelting slag, and simultaneously realizes copper slag depletion and recovery of copper and lead and zinc element fuming.

[0036] The continuous copper smelting method of the present invention aims to improve the overall production efficiency and significantly reduce environmental pollution by optimizing the process flow, reducing the intermediate transportation during the smelting process; it not only breaks through the bottleneck of the traditional smelting process in technology, but also can process complex copper resources and realize efficient resource utilization. The present invention can simplify the process flow, improve production efficiency, reduce environmental pollution, and promote the comprehensive innovation of copper smelting technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0039] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0040] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0042] In each example, unless otherwise specified, the percentages are by mass.

[0043] Example 1

[0044] like Figure 1 As shown, a short-process smelting method for complex copper resources comprises the following steps:

[0045] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 6% of the mass of the complex copper resources and waste circuit boards equivalent to 8% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 15000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.45% Cu and 18.90% S is obtained; a smelting slag containing 3.5% Cu, 0.35% Pb, and 2.04% Zn is obtained.

[0046] (2) The high-grade copper matte is added into the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2400Nm 3 / h, air blowing rate is 15000Nm 3 / h, nitrogen injection rate is 5500Nm 3 / h, the reaction time is 14h; the pure oxygen injection rate during the reduction period is 20Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 300Nm 3 / h, the reaction time is 3.5h, and after the reaction is completed, anode copper containing 99.38% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0047] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and pyrite equivalent to 6% of the mass of the smelting slag and anthracite equivalent to 4.5% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 95.66%, 98.76% and 86.35%, respectively.

[0048] Example 2

[0049] like Figure 1 As shown, a short-process smelting method for complex copper resources comprises the following steps:

[0050] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 7% of the mass of the complex copper resources and waste circuit boards equivalent to 6% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 14000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.25% Cu and 19.23% S is obtained; a smelting slag containing 3.34% Cu, 0.32% Pb, and 2.14% Zn is obtained.

[0051] (2) The high-grade copper matte is added into the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2400Nm 3 / h, air blowing rate is 15000Nm 3 / h, nitrogen injection rate is 5500Nm 3 / h, the reaction time is 14h; the pure oxygen injection rate during the reduction period is 20Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 300Nm 3 / h, the reaction time is 3.5h, and after the reaction is completed, anode copper containing 99.38% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0052] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and pyrite equivalent to 6% of the mass of the smelting slag and anthracite equivalent to 4.5% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 95.45%, 99.06% and 85.47%, respectively.

[0053] Example 3

[0054] like Figure 1 As shown, a short-process smelting method for complex copper resources comprises the following steps:

[0055] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 6% of the mass of the complex copper resources and waste circuit boards equivalent to 8% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 15000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.45% Cu and 18.90% S is obtained; a smelting slag containing 3.5% Cu, 0.35% Pb, and 2.04% Zn is obtained.

[0056] (2) The high-grade copper matte is added to the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2450 Nm 3 / h, air blowing rate is 14800Nm 3 / h, nitrogen injection rate is 5300Nm 3 / h, the reaction time is 14.5h; the pure oxygen injection rate during the reduction period is 25Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 320Nm 3 / h, reaction time 3h, after the reaction is completed, anode copper containing 99.28% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0057] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and pyrite equivalent to 6% of the mass of the smelting slag and anthracite equivalent to 4.5% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 95.66%, 98.76% and 86.35%, respectively.

[0058] Example 4

[0059] like Figure 1 As shown, a short-process smelting method for complex copper resources comprises the following steps:

[0060] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 6% of the mass of the complex copper resources and waste circuit boards equivalent to 8% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 15000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.45% Cu and 18.90% S is obtained; a smelting slag containing 3.5% Cu, 0.35% Pb, and 2.04% Zn is obtained.

[0061] (2) The high-grade copper matte is added into the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2400Nm 3 / h, air blowing rate is 15000Nm 3 / h, nitrogen injection rate is 5500Nm 3 / h, reaction time 14h; pure oxygen injection rate during reduction period is 20Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 300Nm 3 / h, reaction time 3.5h, after the reaction is completed, anode copper containing 99.38% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0062] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and pyrite equivalent to 8% of the mass of the smelting slag and anthracite equivalent to 5% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 96.79%, 98.90% and 85.32%, respectively.

[0063] Example 5

[0064] like Figure 1 As shown, a short-process smelting method for complex copper resources comprises the following steps:

[0065] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 6% of the mass of the complex copper resources and waste circuit boards equivalent to 8% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 15000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.45% Cu and 18.90% S is obtained; a smelting slag containing 3.5% Cu, 0.35% Pb, and 2.04% Zn is obtained.

[0066] (2) The high-grade copper matte is added into the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2400Nm 3 / h, air blowing rate is 15000Nm 3 / h, nitrogen injection rate is 5500Nm 3 / h, reaction time 14h; pure oxygen injection rate during reduction period is 20Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 300Nm 3 / h, reaction time 3.5h, after the reaction is completed, anode copper containing 99.38% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0067] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and calcium sulfate equivalent to 10% of the mass of the smelting slag and anthracite equivalent to 6% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 95.09%, 98.23% and 87.32%, respectively.

[0068] Comparative Example 1

[0069] A short-process smelting method for complex copper resources comprises the following steps:

[0070] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 6% of the mass of the complex copper resources and waste circuit boards equivalent to 8% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 15000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.45% Cu and 18.90% S is obtained; a smelting slag containing 3.5% Cu, 0.35% Pb, and 2.04% Zn is obtained.

[0071] (2) The high-grade copper matte is added into the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2400Nm3 / h, air blowing rate is 15000Nm 3 / h, nitrogen injection rate is 5500Nm 3 / h, reaction time 14h; pure oxygen injection rate during reduction period is 20Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 300Nm 3 / h, reaction time 3.5h, after the reaction is completed, anode copper containing 99.38% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0072] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and pyrite equivalent to 6% of the mass of the smelting slag and anthracite equivalent to 3% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 95.66%, 96.32% and 80.15%, respectively.

[0073] It can be seen that the amount of anthracite added in step (3) of this comparative example is too small, and the recovery rate of lead and zinc is reduced.

[0074] Comparative Example 2

[0075] A short-process smelting method for complex copper resources, comprising the following steps: (changing operating parameters in a blowing-refining furnace)

[0076] (1) 100 kg of complex copper resources are used as raw materials, and the main chemical composition thereof includes 25.13% Cu, 24.32% Fe, 28.14% S, 0.75% Pb, and 2.29% Zn. The complex copper resources are mixed with quartz sand equivalent to 6% of the mass of the complex copper resources and waste circuit boards equivalent to 8% of the mass of the complex copper resources. The mixed materials are added into a smelting furnace through a feeding device, and the temperature is raised to 1200°C. Oxygen is blown into the molten pool using an oxygen gun, and the blowing rate of oxygen is 15000 Nm 3 / h, oxygen enrichment concentration is 75%, oxygen-ore ratio is 147Nm 3 / t. The smelting time is 1 hour. After the reaction is completed, a high-grade copper matte containing 73.45% Cu and 18.90% S is obtained; a smelting slag containing 3.5% Cu, 0.35% Pb, and 2.04% Zn is obtained.

[0077] (2) The high-grade copper matte is added into the blowing-refining furnace through a chute, and quartz sand equivalent to 8% of the mass of the high-grade copper matte is added. The temperature is raised to 1250°C, and the gas is blown into the furnace through an oxygen lance. The pure oxygen blowing rate during the oxidation period is 2800Nm 3 / h, air blowing rate is 18000Nm 3 / h, nitrogen injection rate is 1500Nm 3 / h, the reaction time is 14h; the pure oxygen injection rate during the reduction period is 20Nm 3 / h, air blowing rate is 1300Nm 3 / h, natural gas injection rate is 300Nm 3 / h, the reaction time is 3.5h, and after the reaction is completed, anode copper containing 98.78% Cu is obtained; the obtained blowing slag is returned to the matte making and smelting process.

[0078] (3) The copper smelting slag obtained in step (1) is added to a depletion furnace through a chute for reduction and sulfidation reaction, and pyrite equivalent to 6% of the mass of the smelting slag and anthracite equivalent to 4.5% of the mass of the smelting slag are added to the depletion furnace through a feeding device. After reacting at 1300° C. for 3 hours, copper matte, depleted slag and flue gas are obtained. According to calculation, the recovery rates of copper, lead and zinc (the recovery rate refers to the proportion of copper, lead and zinc recovered from the original slag, the same below) are 95.66%, 98.76% and 86.35%, respectively.

[0079] It can be seen that in this comparative example, the purity of the obtained anode copper decreases as the operating parameters in the blowing-refining furnace in step (2) change.

Claims

1. A short-process smelting method for complex copper resources, characterized in that: The following steps are involved: (1) Mixing complex copper resources with flux and multi-source cold materials, and smelting them under oxygen-rich conditions to obtain high-grade copper matte, smelting slag and flue gas; (2) the high-grade copper matte is mixed with flux and then smelted in a blowing-refining furnace to obtain blowing slag, anode copper and flue gas; (3) The smelting slag obtained in step (1) is combined with a sulfiding agent and a reducing agent to carry out reduction sulfidation to obtain copper matte, depleted slag and flue gas, and valuable metals such as lead and zinc are recovered from the flue gas.

2. The short-process smelting method of complex copper resources according to claim 1 is characterized in that: In step (2), the blown slag is returned to the matte making and smelting process in step (1) as a multi-source cold material; and / or in step (3), the copper matte is returned to the matte making and smelting process in step (1) as a multi-source cold material.

3. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: In step (1), the complex copper resource includes, by weight percentage, 19-30% Cu, 22-28% Fe, 20-30% S, 0.5-1.0% Pb, and 1.5-2.45% Zn; and / or in step (1), the flux is quartz sand, and the addition amount is 4-8% of the mass of the complex copper resource; and / or in step (1), the multi-source cold material is one or more of low-grade copper ore, waste circuit boards, copper-containing sludge, waste copper, and residual cold material, and the addition amount is 5-10% of the mass of the complex copper resource.

4. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: In step (1), oxygen is blown into the furnace under the oxygen-enriched condition, and the blowing rate of oxygen is 10000-30000 Nm 3 / h, oxygen enrichment concentration is 70-82%, oxygen-ore ratio is 145-165Nm 3 / t; and / or in step (1), the smelting temperature is 1180-1250°C; the smelting time is 0.5-2 hours.

5. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: In step (1), the high-grade copper matte comprises 73-78% Cu and 16-21% S in terms of mass percentage; the smelting slag comprises 3-5% Cu, 0.3-1.0% Pb and 1.5-4.0% Zn.

6. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: In step (2), the flux is quartz sand, and the added amount is equivalent to 5-12% of the mass of the high-grade copper matte.

7. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: In step (2), a mixed gas is introduced into the blowing-refining furnace, and the smelting in the blowing-refining furnace includes two processes: an oxidation period and a reduction period; the pure oxygen blowing rate during the oxidation period is 2000-2500 Nm 3 / h, air blowing rate is 14000-16000 Nm 3 / h, nitrogen injection rate is 5000-6000 Nm 3 / h, the reaction time is 12-16h; the pure oxygen injection rate during the reduction period is 20-30 Nm 3 / h, air blowing rate is 1000-1600 Nm 3 / h, natural gas injection rate is 250-450 Nm 3 / h, the reaction time is 2-4h; and / or in step (2), the blowing and refining temperature is 1220-1270°C.

8. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: In step (2), the anode copper comprises 99.01-99.55% Cu in terms of mass percentage.

9. The short-process smelting method for complex copper resources according to claim 1 or 2, characterized in that: The vulcanizing agent is one or more of sulfur, pyrite, calcium sulfate and gypsum slag, and the added amount is 2-15% of the mass of the smelting slag; and / or in step (3), the reducing agent is one or more of coke, anthracite, bituminous coal and biochar, and the added amount is 4-8% of the mass of the smelting slag.

10. The short-process smelting method of complex copper resources according to claim 1 or 2, characterized in that: In step (3), the reduction and sulfidation temperature is 1200-1350° C., and the constant temperature time is 2-5 h; and / or in step (3), valuable metals such as lead and zinc are recovered from the flue gas, wherein the lead recovery rate is greater than 98%, and the zinc recovery rate is greater than 85%.

Citation Information

Cited By

  • Cooperative treatment method for gold smelting and nonferrous smelting waste

    CN120719135A

  • Method for co-processing multi-source copper-based waste through copper concentrate

    CN121450949A

  • Method for treating copper-nickel concentrate rich in platinum group metals

    WO2026200335A1