Comprehensive utilization method and system of zinc concentrate calcine

CN118910422APending Publication Date: 2024-11-08SHAANXI ZHONGYAN DIHUAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959844.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

这种方法虽然提取了硅,但其锌的总浸出率基本在89%~92%,总浸出率仍比较低,而残渣产率达到了55%~65%,残渣产率又太高,整体来说对于原料内各种元素的利用率还是有限,造成大量元素的浪费;且该方法两段浸出时间分别要求在120分钟~180分钟、120分钟~140分钟,总浸出时间太长,不利于工业化应用

Benefits of technology

[0023] The comprehensive utilization method of zinc concentrate roasting sand provided by the present invention, on the one hand, improves the comprehensive utilization rate of zinc concentrate roasting sand, greatly reduces the slag production rate, and the generated residues have higher recycling value. Specifically, Land, the present invention can simultaneously provide Take zinc, silicon, iron and other elements. Even if a small amount of zinc remains in the first acid leaching residue in the first acid leaching, it can be leached into the third acid leaching liquid in the subsequent steps, and then enter the third acid leaching liquid. Four acid leaches, and then returned to the leaching of zinc concentrate roasting sand Therefore, the zinc in the zinc concentrate roasting sand will not be wasted, so that the total leaching rate of zinc can reach more than 98%; at the same time, the silica gel obtained from the silicon element and the goethite obtained from the iron element are separated. The purity can reach more than 99% and 98% respectively, and can be directly used in industry; at the same time, the method of the present invention can also highly enrich a small amount of elements lead and silver in the zinc concentrate roasting sand, and obtain the second acid leaching The slag can be used as raw material for extracting lead and silver. On the other hand, the two leaching times in the entire process of the method of the present invention are 10 minutes to 40 minutes and 1 hour to 3 hours respectively. The leaching time is greatly shortened, and the leaching efficiency is high, which is conducive to wide application in industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910422A_ABST
    Figure CN118910422A_ABST
Patent Text Reader

Abstract

The invention relates to a comprehensive utilization method and system of zinc concentrate calcine, the method comprises the following steps: firstly, mixing the zinc concentrate calcine with a sulfuric acid solution with the initial concentration of 100g / L-200g / L, controlling the end ph value of the solution to be 3-5, reacting for 10-40 minutes at the temperature of 25-55 DEG C, continuously reacting the obtained first pickle liquor at the temperature of 50-90 DEG C to obtain silica gel and second pickle liquor, s10, adding the obtained first acid leaching residues into a sulfuric acid solution with the initial concentration of 200g / L-300g / L, adding the obtained third acid leaching solution into a sulfuric acid solution with the pH value of 3-3.5, controlling the pH value of the solution to be 3-3.5 at the same time, obtaining a fourth acid leaching solution and goethite, and returning the fourth acid leaching solution to the step S10 after adjusting the sulfuric acid concentration so as to be used for leaching zinc concentrate calcine. According to the method, efficient comprehensive utilization of the zinc concentrate calcine can be achieved, the process time is short, and the method can be widely applied to industrial treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a comprehensive utilization method and system of zinc concentrate roasted sand. Background Art

[0002] Zinc concentrate roasted sand is the product obtained after zinc concentrate is roasted. It contains major elements such as zinc, silicon, iron and trace elements such as lead and silver, and is used for zinc smelting. The existing zinc smelting method adopts three-stage leaching, namely neutral leaching, weak acid leaching and low acid leaching. The zinc smelting slag produced by this method is not only huge in volume (slag production rate is more than 40%), but also hazardous waste slag containing heavy metal elements such as cadmium and lead. It must be treated by pyrolysis to eliminate heavy metal elements such as cadmium and lead and meet the general solid waste discharge standards. In the production process, silicon is regarded as a "harmful element" in the entire zinc smelting process. The presence of silicon dioxide not only directly affects the leaching slag rate, but also affects the clarification time and filtration difficulty of the leachate, and even restricts the entire process time and production operation efficiency.

[0003] Some zinc smelting methods also use two-stage leaching and silicon extraction, such as the prior art CN1477217A, which uses neutral leaching and low-acid leaching. First, zinc is leached through neutral leaching, and iron and silicon are hydrolyzed and precipitated in acid leaching residues. Then, the acid leaching residues are subjected to low-acid leaching to separate iron and silicon. Although this method extracts silicon, its total zinc leaching rate is basically 89% to 92%, which is still relatively low, and the residue yield reaches 55% to 65%, which is too high. Overall, the utilization rate of various elements in the raw materials is still limited, resulting in a large amount of waste of elements; and the two-stage leaching time of this method is required to be 120 minutes to 180 minutes and 120 minutes to 140 minutes respectively, and the total leaching time is too long, which is not conducive to industrial application. Summary of the invention

[0004] Based on the above situation, the main purpose of the present invention is to provide a method and system for comprehensive utilization of zinc concentrate roasted sand, so as to achieve efficient comprehensive utilization of zinc concentrate roasted sand, and the process time is short, and it can be widely used in industrial processing.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] The first aspect of the present invention provides a method for comprehensive utilization of zinc concentrate roasted sand, wherein the zinc concentrate roasted sand comprises major elements zinc, silicon, iron and minor elements lead and silver, and the content of zinc is greater than that of iron, and the content of iron is greater than that of silicon; the method comprises the steps of:

[0007] S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution having an initial concentration of 100 g / L to 200 g / L, controlling the end point pH value of the solution to be 3 to 5, stirring at a temperature of 25° C. to 55° C. for 10 to 40 minutes, filtering and separating to obtain a first acid leaching solution and a first acid leaching residue; wherein the zinc element and the silicon element in the zinc concentrate roasted sand are leached into the first acid leaching solution, and the iron element, the lead element and the silver element remain in the first acid leaching residue;

[0008] S20: continuing to react the first acid leaching solution at a temperature of 50° C. to 90° C., and then filtering and separating to obtain a second acid leaching solution and silica gel, wherein the zinc element in the first acid leaching solution is leached into the second acid leaching solution;

[0009] S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 200 g / L to 300 g / L, reacting for 1 to 3 hours, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue; wherein the iron element in the first acid leaching residue is leached into the third acid leaching solution; and the lead element and the silver element remain in the second acid leaching residue;

[0010] S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, while controlling the pH value of the solution to be in the range of 3 to 3.5, so that the iron element in the third acid leaching solution is fully reacted to generate goethite, and filtering and separating to obtain a fourth acid leaching solution and goethite;

[0011] S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to the initial concentration of sulfuric acid in step 10, return to step S10.

[0012] Optionally, in step S10, the roasted zinc concentrate is added to a sulfuric acid solution with an initial concentration of 100 g / L to 200 g / L, stirred to mix the two, and the pH value of the solution at the end point is controlled to be 3 to 5 by controlling the amount of the roasted zinc concentrate added.

[0013] Optionally, in step S20, the first acid leaching solution is stirred at a temperature of 50° C. to 90° C. for 0.5 hour to 3 hours, and then filtered and separated.

[0014] Optionally, the step S20 further includes the step of first treating the second acid leaching liquid through a purification step, and then electrolyzing zinc.

[0015] Optionally, in step S30, the first acid leaching residue is added to the sulfuric acid solution at a temperature of 80° C. to 110° C. while stirring.

[0016] Optionally, the first acid leaching residue further contains residual unleached zinc element;

[0017] In the step S30, the amount of the sulfuric acid solution is greater than the amount required to leach the iron and zinc in the first acid leaching residue, so that the iron and zinc elements in the first acid leaching residue are leached into the third acid leaching solution.

[0018] Optionally, in step S40, the pH value of the solution is controlled to be in the range of 3 to 3.5 by adding zinc oxide.

[0019] Optionally, in step S40, the third acid leaching solution is slowly added to the sulfuric acid solution at a temperature of 75° C. to 95° C., and the pH value of the solution is controlled to be in the range of 3 to 3.5 by controlling the addition rate of the third acid leaching solution and the addition rate of zinc oxide.

[0020] Optionally, in step S40, after all of the third acid leaching liquid is added to the sulfuric acid solution, stirring is performed for 10 to 20 minutes, and then filtering and separating is performed.

[0021] The second aspect of the present invention provides a comprehensive utilization system of zinc concentrate roasted sand, which is used to implement any of the above-mentioned comprehensive utilization methods of zinc concentrate roasted sand; comprising:

[0022] A mixed reaction device for acid leaching reaction in steps S10, S20, S30 and S40, and a filtration separation device for filtration separation in steps S10, S20, S30 and S40.

[0023] The comprehensive utilization method of zinc concentrate roasted sand provided by the present invention improves the comprehensive utilization rate of zinc concentrate roasted sand, greatly reduces the slag production rate, and the generated residues have higher recycling value. Specifically, the present invention can simultaneously extract zinc, silicon, iron and other elements. Even if a small amount of zinc element remains in the first acid leaching residue in the first acid leaching, it can be leached into the third acid leaching solution in the subsequent steps, and then enter the fourth acid leaching solution, and then return to the leaching process of the zinc concentrate roasted sand for enrichment. Therefore, zinc in the zinc concentrate roasted sand will not be wasted, so that the total leaching rate of zinc can reach more than 98%; the purity of silica gel obtained by separating silicon element and goethite obtained by separating iron element can reach more than 99% and 98% respectively, and can be directly applied to industry; at the same time, the method of the present invention can also highly enrich the small amount of lead and silver elements in the zinc concentrate roasted sand, and the obtained second acid leaching residue can be used as a raw material for extracting lead and silver. On the other hand, the two leaching times in the whole process of the method of the present invention are respectively 10 minutes to 40 minutes and 1 hour to 3 hours, the leaching time is greatly shortened, and the leaching efficiency is high, which is conducive to wide application in industry.

[0024] Other beneficial effects of the present invention will be explained in the specific implementation manner through the introduction of specific technical features and technical solutions. Through the introduction of these technical features and technical solutions, those skilled in the art should be able to understand the beneficial technical effects brought about by the technical features and technical solutions. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings.

[0026] Figure 1 A schematic flow chart of an implementation method of the comprehensive utilization method of zinc concentrate provided by the present invention;

[0027] Figure 2 This is a schematic diagram of the changes in components in each step in one embodiment of the method for comprehensive utilization of zinc concentrate provided by the present invention. DETAILED DESCRIPTION

[0028] The present invention is described below based on embodiments, but the present invention is not limited to these embodiments. In the following detailed description of the present invention, some specific details are described in detail. In order to avoid confusing the essence of the present invention, known methods, processes, procedures, and components are not described in detail.

[0029] In addition, persons of ordinary skill in the art will appreciate that the drawings provided herein are for illustration purposes and are not necessarily drawn to scale.

[0030] Unless the context clearly requires otherwise, throughout the specification and claims, the words "include", "comprising" and similar words should be interpreted in an inclusive sense rather than an exclusive or exhaustive sense; that is, in the sense of "including but not limited to".

[0031] In the description of the present invention, it should be understood that the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. In addition, in the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0032] In the description of the present invention, "content" refers to mass percentage; M in M2SiO4 and MSO4 represents a certain cation, such as Ca, Mg, etc.; "aq" in the reaction equations of each step reaction represents a solution.

[0033] The present invention provides a comprehensive utilization method of zinc concentrate roasted sand, which can be used in the treatment of zinc concentrate roasted sand. Wherein, zinc concentrate roasted sand is a product obtained after zinc concentrate is roasted, which includes major elements zinc, silicon, iron and a small amount of elements lead and silver, and the content of zinc element is greater than the content of iron element, and even the content of zinc element is greater than 2 times the content of iron element, and the content of iron element is greater than the content of silicon element. It should be noted that the zinc element in the zinc concentrate roasted sand mainly exists in the form of zinc oxide (ZnO), and a part of zinc exists together with a part of iron element in the form of zinc ferrite (ZnFe2O4), the silicon element mainly exists in the form of silicate (M2SiO4), and a part of iron element exists in the form of iron oxide (Fe2O3), and the lead element, silver element, etc. mainly exist in the form of lead oxide and silver oxide, respectively. Specifically, in the zinc concentrate roasted sand, the Zn content is 45% to 60%, the silicon content is 3% to 5%, the iron content is 10% to 15%, the Pb content is 1% to 2%, and the Ag content can basically reach 130g / t to 200g / t. Of course, the zinc concentrate roasted sand contains many other elements, and their contents are relatively small, such as Ca content of 1.5% to 2.5%, Mg content of 0.5% to 1%, Al content of 0.3% to 0.7%, Cd content of 0.4% to 0.8%, Cu content of 0.2% to 0.4%, etc. These elements also mainly exist in the form of their oxides.

[0034] like Figure 1-Figure 2 As shown, the comprehensive utilization method of zinc concentrate roasted sand comprises the steps of:

[0035] S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution with an initial concentration of 100 g / L to 200 g / L, controlling the end point pH value of the solution to be 3 to 5, stirring at a temperature of 25° C. to 55° C. for 10 to 40 minutes, filtering and separating to obtain a first acid leaching solution and a first acid leaching residue; wherein zinc and silicon elements in the zinc concentrate roasted sand are leached into the first acid leaching solution, and iron, lead and silver elements are retained in the first acid leaching residue.

[0036] In step S10, the first acid leaching reaction is carried out, and the initial concentration of the sulfuric acid solution is 100 g / L to 200 g / L, such as 100 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L, 180 g / L, 190 g / L or 200 g / L, etc. In the process of mixing the zinc concentrate roasted sand and the sulfuric acid solution, the endpoint pH value of the solution is controlled to be 3 to 5, such as the endpoint pH value of the solution is 3, 3.1, 3.3, 3.5, 3.7, 3.9, 4, 4.2, 4.4, 4.5, 4.7, 4.8, 4.9 or 5.0, etc. The temperature of the entire reaction system is controlled at 25°C to 55°C, such as 25°C, 26°C, 28°C, 30°C, 35°C, 38°C, 40°C, 43°C, 45°C, 48°C, 50°C, 52°C, 54°C or 55°C, and the zinc in the zinc concentrate roasted sand is leached as much as possible by stirring. At the same time, the reaction time is controlled to be 10 minutes to 40 minutes, such as 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, so that the zinc in the zinc concentrate roasted sand is leached as much as possible, and the leaching of iron is avoided, that is, the first acid leaching solution obtained substantially does not contain iron. In this process, the zinc oxide in the zinc concentrate roasted sand is substantially leached, while the zinc ferrite remains in the first acid leaching residue. In general, in the first acid leaching reaction of the zinc concentrate roasted sand, the pH value of the solution, the temperature of the reaction system and the reaction time are controlled so that the zinc and silicon in the zinc concentrate roasted sand are leached into the first acid leaching solution as much as possible, while the iron is not leached. Then the first acid leaching solution and the first acid leaching residue are separated by filtration. The first acid leaching solution includes most of the zinc and silicon in the zinc concentrate roasted sand and basically does not contain iron, while the first acid leaching residue contains elements such as iron, lead and silver.

[0037] Among them, the reaction equation of the chemical reaction mainly occurring in the first acid leaching reaction is as follows:

[0038] M2SiO4+2H2SO4+aq=H4SiO4+2MSO4+aq (M represents a certain cation, such as Ca, Mg, etc.);

[0039] ZnO+H2SO4+aq=ZnSO4+H2O+aq.

[0040] It should be noted that in the above reaction equation, each element in the zinc concentrate roasted sand is expressed as a reactant phase in the form of oxides.

[0041] S20: continuing to react the first acid leaching solution at a temperature of 50° C. to 90° C., and then filtering and separating to obtain a second acid leaching solution and silica gel, wherein the zinc element in the first acid leaching solution is leached into the second acid leaching solution.

[0042] In step S20, the first acid leaching solution is further reacted in a reaction system with a relatively high temperature to remove silicon from the first acid leaching solution. Specifically, the orthosilicic acid H4SiO4 generated in step S10 is polymerized at a temperature of 50°C to 90°C to form silica gel, such as at a temperature of 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C. After the silica gel is formed, the second acid leaching solution obtained by filtration and separation basically does not contain silicon, thereby increasing the zinc content in the second acid leaching solution, which can be used as a raw material for zinc smelting, such as directly as a raw material for electrolytic zinc. Of course, in the subsequent electrolytic zinc process, a small amount of elements such as Ca, Mg, Cu, and Cd in the second acid leaching solution can be further removed through a purification step (described in detail below). The obtained silica gel is a qualified product after simple rinsing and drying, and can be applied to various fields such as industry.

[0043] The equation for the main reaction occurring in step S20 is as follows:

[0044] nH4SiO4=nSiO2·(n+1)H2O+(n-1)H2O.

[0045] S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 200 g / L to 300 g / L, reacting for 1 to 3 hours, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue; wherein the iron element in the first acid leaching residue is leached into the third acid leaching solution; and the lead element and the silver element remain in the second acid leaching residue.

[0046] In this step, a second acid leaching reaction is carried out, and the first acid leaching residue is added to a sulfuric acid solution with an initial concentration of 200 g / L to 300 g / L, such as an initial concentration of the sulfuric acid solution of 200 g / L, 220 g / L, 240 g / L, 250 g / L, 270 g / L, 290 g / L or 300 g / L. In step S30, the first acid leaching residue reacts with sulfuric acid for 1 hour to 3 hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, so that the iron element in the first acid leaching residue is leached as much as possible, that is, all the iron elements in the zinc concentrate roasted sand are basically leached into the third acid leaching solution. At the same time, if part of the zinc is not leached in the first acid leaching reaction, it can also be leached in this acid leaching reaction (described in detail below), that is, in the second acid leaching reaction, the iron and residual zinc in the first acid leaching residue can be basically leached, while lead and silver are left in the second acid leaching residue, wherein the main components of the third acid leaching solution include all the iron and residual zinc in the zinc concentrate roasted sand, and basically do not contain lead and silver. That is to say, the iron element and the residual zinc element (i.e., the element not leached in the first acid leaching reaction) in the zinc concentrate roasted sand are basically all leached into the third acid leaching solution, while the small amount of lead and silver elements in the zinc concentrate roasted sand are basically all left in the second acid leaching residue, so that the lead and silver elements in the second acid leaching residue are enriched relative to the content in the initial zinc concentrate roasted sand, and the lead element can be enriched by more than 19 times, and the silver element can be enriched by more than 5 times. Therefore, the second acid leaching residue can be used as a raw material for extracting lead and silver elements. Among them, the reaction equation of the main chemical reaction occurring in the second acid leaching reaction is as follows:

[0047] ZnFe2O4+4H2SO4+aq=ZnSO4+Fe2(SO4)3+4H2O+aq.

[0048] Fe2O3+3H2SO4+aq=Fe2(SO4)3+3H2O+aq.

[0049] S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, while controlling the pH value of the solution to be in the range of 3 to 3.5, so that the iron element in the third acid leaching solution fully reacts to generate goethite, filtering and separating, and obtaining a fourth acid leaching solution and goethite.

[0050] In this step, the third acid leaching solution is added to a sulfuric acid solution with a pH value of 3 to 3.5, such as a sulfuric acid solution with a pH value of 3, 3.1, 3.2, 3.3, 3.4 or 3.5, and the pH value of the solution is controlled in the range of 3 to 3.5 during the entire reaction process, such as the pH value of the solution can be controlled to be 3, 3.1, 3.2, 3.3, 3.4 or 3.5, etc. It should be noted that the pH value of the reaction system can be controlled in the range of 3 to 3.5, and is not necessarily limited to a specific point value. In this way, by controlling the pH value of the solution, the iron element in the third acid leaching solution can be fully hydrolyzed, so that the iron element in the zinc concentrate roasted sand can basically form a precipitate, and then be filtered and separated in the filtration, that is, the precipitate obtained by filtration and separation is goethite, and the liquid is the fourth acid leaching solution. The residual zinc element enters the third acid leaching solution in the second acid leaching reaction, and will remain in the fourth acid leaching solution in step S40. Among them, the equation of the main chemical reaction occurring in step S40 is as follows:

[0051] Fe 3+ +2H2O=FeOOH↓+3H + .

[0052] S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to the initial concentration of sulfuric acid, return to step S10.

[0053] In this step, the fourth acid leaching solution still contains a large amount of sulfuric acid, and the concentration of the sulfuric acid can be adjusted first, and then it is returned to step S10, that is, the sulfuric acid concentration of the fourth acid leaching solution is adjusted to be consistent with the initial sulfuric acid concentration in step S10, and then used as the sulfuric acid in step S10 for the first acid leaching reaction. In this way, even if there is residual zinc element in the first acid leaching reaction, it can be returned to the next first acid leaching reaction again to participate in the leaching of zinc element in the zinc concentrate roasted sand, so that the zinc element in the zinc concentrate roasted sand will not be wasted.

[0054] The comprehensive utilization method of zinc concentrate roasted sand provided by the present invention comprises the following steps: in the first acid leaching of the zinc concentrate, by controlling the end point pH value of the solution to be 3-5, and reacting for 10-40 minutes at a temperature of 25-55°C, the zinc and silicon elements in the zinc concentrate roasted sand can be leached into the first acid leaching solution as much as possible, while the iron element will not be leached; then, the first acid leaching solution is allowed to continue to react at a higher temperature of 50-90°C to separate silicon, and the second acid leaching solution from which silicon is removed can be directly used as a raw material for electrolytic zinc, and the separated silica gel can also be directly used in industry. The first acid leaching residue can remove the lead and silver elements in the second acid leaching residue through the second acid leaching reaction, and the separated second acid leaching residue containing lead and silver elements can be directly used as a raw material for extracting lead and silver because the lead and silver elements are enriched by 19 times and 5 times or more relative to the content of the zinc concentrate roasted sand respectively; then, the third acid leaching liquid from which the lead and silver have been removed is added to the sulfuric acid solution, and the pH value of the solution is controlled in the range of 3 to 3.5 so that the iron element in the third acid leaching liquid is precipitated as much as possible to obtain goethite, thereby completing the extraction of iron; the separated fourth acid leaching liquid contains sulfuric acid, and the sulfuric acid concentration can be adjusted and then returned to step S10, and no waste of sulfuric acid is caused. Of course, even if there is a small amount of residual zinc element in the zinc concentrate roasted sand that has not been leached, it can be leached again in the first acid leaching reaction of the zinc concentrate roasted sand with the fourth acid leaching liquid, so this part of the zinc element can also be fully utilized.

[0055] In summary, the comprehensive utilization method of zinc concentrate roasted sand of the present invention, on the one hand, improves the comprehensive utilization rate of zinc concentrate roasted sand, greatly reduces the slag production rate, and the generated residues have higher recycling value. Specifically, the present invention can simultaneously extract zinc, silicon, iron and other elements. Even if a small amount of zinc element remains in the first acid leaching residue in the first acid leaching, it can be leached into the third acid leaching solution in the subsequent steps, and then enter the fourth acid leaching solution, and then return to the leaching process of the zinc concentrate roasted sand for enrichment. Therefore, zinc in the zinc concentrate roasted sand will not be wasted, so that the total leaching rate of zinc can reach more than 98%; at the same time, the purity of silica gel obtained by separating silicon element and goethite obtained by separating iron element can reach more than 99% and 98%, respectively, and can be directly applied to industry; and the method of the present invention can also highly enrich the small amount of lead and silver in the zinc concentrate roasted sand, and the obtained second acid leaching residue can be used as a raw material for extracting lead and silver. On the other hand, the two leaching times in the whole process of the method of the present invention are respectively 10 minutes to 40 minutes and 1 hour to 3 hours, the leaching time is greatly shortened, and the leaching efficiency is high, which is conducive to wide application in industry.

[0056] In some embodiments, in the above step S40, sulfuric acid is added to the third acid leaching solution, but the concentration of iron ions in the solution in this way is high, and iron hydroxide colloid is generated when sulfuric acid solution is added, which increases the difficulty of subsequent separation because iron hydroxide colloid is not easy to filter. In the present invention, by adding the third acid leaching solution to the sulfuric acid solution, the concentration of iron ions in the solution is always low, thereby ensuring that goethite is generated, reducing the difficulty of subsequent filtration and separation. The comprehensive utilization method of the present invention is simpler and easier to implement, which is further conducive to wide application in industry.

[0057] As mentioned above, in addition to the zinc, silicon, iron, lead, and silver elements listed in the above steps, there are also some other components in the zinc concentrate roasted sand, such as calcium, magnesium, cadmium, aluminum and other elements. Among them, calcium, magnesium, cadmium, and copper are also basically present in the form of oxides in the zinc concentrate roasted sand, and will be leached in the first acid leaching reaction (i.e., step S10). That is to say, calcium, magnesium, cadmium, and copper will be leached into the first acid leaching solution in the first acid leaching reaction, and then after silicon removal in step S20, they will remain in the second acid leaching solution. Among them, the chemical reaction equations of calcium, magnesium, cadmium, and copper oxides in the first acid leaching reaction are as follows:

[0058] CaO+H2SO4+aq=CaSO4(slightly soluble)+H2O+aq;

[0059] MgO+H2SO4+aq=MgSO4+H2O+aq;

[0060] CdO+H2SO4+aq=CdSO4+H2O+aq;

[0061] CuO+H2SO4+aq=CuSO4+H2O+aq.

[0062] Among them, a small amount of aluminum in the zinc concentrate roasted sand mainly exists in the form of Al2O3. This part of aluminum basically remains in the first acid leaching residue in the first acid leaching reaction, and is leached together with iron in the second acid leaching reaction (i.e., step S30), that is, a small amount of aluminum in the zinc concentrate roasted sand will eventually enter the second acid leaching solution. Specifically, the chemical reaction equation of this part of aluminum in the second acid leaching reaction (i.e., step S30) is as follows:

[0063] Al2O3+3H2SO4+aq=Al2(SO4)3+3H2O+aq.

[0064] Wherein, in the above step S10, the pH value of the solution endpoint is controlled to be 3 to 5, which can be adjusted by adding other substances, such as zinc oxide. In step S10, the zinc concentrate roasted sand can be added to the sulfuric acid solution to mix the two, or the sulfuric acid solution can be added to the zinc concentrate roasted sand to mix the two. In a preferred embodiment of the present invention, step S10 specifically adds the zinc concentrate roasted sand to the sulfuric acid solution, and controls the amount of zinc concentrate roasted sand added to achieve a solution endpoint pH value of 3 to 5. Specifically, in step S10, the zinc concentrate roasted sand is added to the sulfuric acid solution with an initial concentration of 100g / L to 200g / L, stirred to mix the two, and the pH value of the solution endpoint is 3 to 5 by controlling the amount of zinc concentrate roasted sand added. In this way, there is no need to add other substances, which can reduce the consumables in the comprehensive utilization process of zinc concentrate roasted sand and improve the utilization rate of raw materials.

[0065] In step S20, the orthosilicic acid (H4SiO4) in the first acid leaching solution can be gradually polymerized to form a colloid, i.e., silica gel, at a temperature of 50°C to 90°C, and the solution is filtered when no more colloid is formed by observation. In a preferred embodiment, in order to increase the polymerization rate of silica gel, in step S20, the first acid leaching solution is stirred at a temperature of 50°C to 90°C for 0.5 to 3 hours, and then filtered and separated, that is, the first acid leaching solution is stirred at 50°C to 90°C for about 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, and then filtered and separated, the silicon in the first acid leaching solution has basically been polymerized into silica gel, and the silicon in the first acid leaching solution can be removed cleanly, thereby improving the purity of subsequent iron extraction and improving the utilization rate of silicon in zinc concentrate roasted sand.

[0066] In the hydrometallurgical zinc smelting, zinc is produced by electroplating after step S20. The second acid leaching solution obtained by the above method may also contain a small amount of elements such as calcium, magnesium, copper, and cadmium. Therefore, in order to improve the purity of the prepared zinc, in a preferred embodiment, after step S20, the second acid leaching solution is further treated by a purification step, and then electrolytic zinc is produced. By adding this step, other components in the first acid leaching solution except zinc can be removed as much as possible, especially calcium, magnesium, copper, cadmium and other components, thereby improving the purity of the prepared zinc product. Among them, the purification step can be any method in the prior art, and can be specifically set according to the elements to be removed, such as reducing the solubility of calcium sulfate and magnesium by cooling to make them crystallize and precipitate, and removing copper and cadmium by zinc powder replacement method.

[0067] In order to improve the efficiency of the second acid leaching reaction, in step S30, the first acid leaching residue is added to the sulfuric acid solution at a temperature of 80°C to 110°C while stirring. That is, in step S30, the temperature of the reaction system is controlled to be 80°C to 110°C, such as 80°C, 85°C, 90°C, 95°C, 100°C, 105°C or 110°C, and the first acid leaching residue is added to the sulfuric acid solution while stirring, and the stirring is continued after the first acid leaching residue is added, so that the iron in the first acid leaching residue can be completely leached. In this step, the amount of sulfuric acid solution can be determined in advance by measuring the iron content in the first acid leaching residue to ensure that the amount of sulfuric acid solution selected is greater than the required amount for leaching iron.

[0068] As mentioned above, some zinc elements may not be leached in the first acid leaching reaction, that is, the first acid leaching residue also includes residual zinc elements that have not been leached; at this time, in step S30, the amount of sulfuric acid solution is greater than the amount required to leach the iron and zinc in the first acid leaching residue, so that the iron and zinc elements in the first acid leaching residue are leached into the third acid leaching solution. In other words, the amount of sulfuric acid selected in step S30 is greater than the amount required to leach the iron and zinc in the first acid leaching residue, so as to ensure that the iron and zinc in the zinc concentrate roasted sand can be basically leached. Among them, the reaction equation for zinc leaching is as follows:

[0069] ZnO+H2SO4+aq=ZnSO4+H2O+aq.

[0070] Among them, in the above-mentioned step S50, some embodiments control the pH value of the solution in the range of 3 to 3.5 by adding zinc concentrate roasted sand, etc. However, since the zinc concentrate roasted sand contains silicon, it will also participate in the reaction to form a colloid in this step, affecting the subsequent separation of goethite. In a preferred embodiment, in step S40, the pH value of the solution is controlled in the range of 3 to 3.5 by adding zinc oxide. The pH value of the solution is adjusted by zinc oxide, and no additional components are added, and the added zinc element will not be wasted, but will enter the fourth acid leaching solution. When it returns to step S10, it will be leached and enter the second acid leaching solution and then used as a raw material for zinc extraction. Among them, the equation for the chemical reaction that occurs when zinc oxide is added to adjust the pH value is as follows:

[0071] ZnO+H2SO4+aq=ZnSO4+H2O+aq.

[0072] Further, in the above step S40, the third acid leaching solution is slowly added to the sulfuric acid solution at a temperature of 75°C to 95°C, and the pH value of the solution is controlled in the range of 3 to 3.5 by controlling the addition rate of the third acid leaching solution and the addition rate of zinc oxide. That is, in step S40, the temperature of the reaction system is 75°C to 95°C, such as 75°C, 80°C, 85°C, 90°C or 95°C, and the third acid leaching solution is slowly added to the sulfuric acid solution to control the pH value of the solution, thereby ensuring that the iron ions can be fully hydrolyzed and no iron hydroxide colloid is generated.

[0073] In step 40, the third acid leaching solution is added to the sulfuric acid solution while being stirred so that the iron ions react fully. After the third acid leaching solution is completely added to the sulfuric acid solution, stirring is continued for 10 to 20 minutes, and then filtering and separating is performed. For example, after the third acid leaching solution is completely added to the sulfuric acid solution, stirring is continued for 10 minutes, 12 minutes, 14 minutes, 15 minutes, 16 minutes, 18 minutes or 20 minutes, so that the iron ions in the third acid leaching solution are hydrolyzed as much as possible, thereby improving the utilization rate of the iron element in the zinc concentrate roasted sand.

[0074] In the above steps S10, S20, S30 and S40, each step may be heated by a water bath so that the temperature of the reaction system in each step can be maintained within a corresponding temperature range.

[0075] The present invention also provides a comprehensive utilization system of zinc concentrate roasted sand, which is used to implement the comprehensive utilization method of zinc concentrate roasted sand described in any of the above embodiments, and the comprehensive utilization system includes: a mixed reaction device for acid leaching reaction in steps S10, S20, S30 and S40, and a filtration separation device for filtration separation in steps S10, S20, S30 and S40. Further, the mixed reaction device includes a heating device, which can be used to heat the solution in the reaction system.

[0076] The above-mentioned comprehensive utilization method of the present invention is described below with specific embodiments.

[0077] Example 1

[0078] In the zinc concentrate roasted sand of this embodiment, the Zn content is 56%, the silicate content is 3.31%, and the Fe2O3 content is 12.35%. The neutralization and utilization method of the zinc concentrate roasted sand comprises the following steps:

[0079] S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution with an initial concentration of 150 g / L, controlling the end point pH value of the solution to be 3.5-4, stirring at a temperature of 50° C. for 40 minutes, and filtering and separating to obtain a first acid leaching solution and a first acid leaching residue;

[0080] S20: continuing the reaction of the first acid leaching solution at a temperature of 70° C. for 60 minutes, and then filtering and separating to obtain a second acid leaching solution and silica gel;

[0081] S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 250 g / L, reacting at 105° C. for 2 hours, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue;

[0082] S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, stirring at 95° C., and adding zinc oxide powder to control the pH value of the solution to be in the range of 3 to 3.5, until all the third acid leaching solution is added, continuing stirring for 10 minutes, filtering and separating, and obtaining a fourth acid leaching solution and goethite;

[0083] S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to 150 g / L, return to step S10.

[0084] After analysis and detection, in step S10, the leaching rate of zinc reached 88.52%, the leaching rate of silicon reached 85.23%, and the leaching rate of iron reached 1.19%; after step S30, the total leaching rate of zinc reached 98.75%, the total leaching rate of silicon reached 86.39%, and the total leaching rate of iron reached 95.75%.

[0085] Example 2

[0086] The zinc concentrate roasted sand of this embodiment has the same composition as that of embodiment 1, and its comprehensive utilization method comprises the steps of:

[0087] S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution with an initial concentration of 100 g / L, controlling the end point pH value of the solution to be 3-3.5, stirring at a temperature of 35° C. for 10 minutes, and filtering and separating to obtain a first acid leaching solution and a first acid leaching residue;

[0088] S20: continuing the reaction of the first acid leaching solution at a temperature of 50° C. for 180 minutes, and then filtering and separating to obtain a second acid leaching solution and silica gel;

[0089] S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 300 g / L, reacting at 100° C. for 2 hours, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue;

[0090] S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, stirring at 75° C., and adding zinc oxide powder to control the pH value of the solution to be in the range of 3 to 3.5, until all the third acid leaching solution is added, continuing stirring for 20 minutes, filtering and separating, and obtaining a fourth acid leaching solution and goethite;

[0091] S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to 100 g / L, return to step S10.

[0092] After analysis and detection, in step S10, the leaching rate of zinc reached 91.15%, the leaching rate of silicon reached 87.81%, and the leaching rate of iron reached 2.21%; after step S30, the total leaching rate of zinc reached 99.12%, the total leaching rate of silicon reached 90.51%, and the total leaching rate of iron reached 93.84%.

[0093] Example 3

[0094] In the zinc concentrate roasted sand of this embodiment, the Zn content is 58%, the silicate content is 4.22%, and the Fe2O3 content is 11.19%. The neutralization and utilization method of the zinc concentrate roasted sand comprises the following steps:

[0095] S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution having an initial concentration of 120 g / L, controlling the end point pH value of the solution to be 4.5-5, stirring at a temperature of 55° C. for 40 minutes, and filtering and separating to obtain a first acid leaching solution and a first acid leaching residue;

[0096] S20: continuing the reaction of the first acid leaching solution at a temperature of 80° C. for 60 minutes, and then filtering and separating to obtain a second acid leaching solution and silica gel, wherein the zinc element in the first acid leaching solution is leached into the second acid leaching solution;

[0097] S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 300 g / L, reacting at 110° C. for 1 hour, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue;

[0098] S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, stirring at 90° C., and adding zinc oxide powder to control the pH value of the solution to be in the range of 3 to 3.5, until all the third acid leaching solution is added, continuing stirring for 15 minutes, filtering and separating, and obtaining a fourth acid leaching solution and goethite;

[0099] S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to 120 g / L, return to step S10.

[0100] After analysis and detection, in step S10, the leaching rate of zinc reached 90.42%, the leaching rate of silicon reached 86.51%, and the leaching rate of iron reached 1.75%; after step S30, the total leaching rate of zinc reached 98.23%, the total leaching rate of silicon reached 89.23%, and the total leaching rate of iron reached 94.83%.

[0101] Example 4

[0102] The zinc concentrate roasted sand of this embodiment has the same composition as that of embodiment 3, and its comprehensive utilization method comprises the steps of:

[0103] S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution with an initial concentration of 200 g / L, controlling the end point pH value of the solution to be 3-4, stirring at a temperature of 25° C. for 30 minutes, and filtering and separating to obtain a first acid leaching solution and a first acid leaching residue;

[0104] S20: continuing the reaction of the first acid leaching solution at a temperature of 90° C. for 30 minutes, and then filtering and separating to obtain a second acid leaching solution and silica gel;

[0105] S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 200 g / L, reacting at 80° C. for 3 hours, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue;

[0106] S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, stirring at 80° C., and adding zinc oxide powder to control the pH value of the solution to be in the range of 3 to 3.5, until all the third acid leaching solution is added, continuing stirring for 15 minutes, filtering and separating, and obtaining a fourth acid leaching solution and goethite;

[0107] S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to 200 g / L, return to step S10.

[0108] After analysis and detection, in step S10, the leaching rate of zinc reached 89.96%, the leaching rate of silicon reached 88.17%, and the leaching rate of iron reached 1.98%; after step S30, the total leaching rate of zinc reached 99.07%, the total leaching rate of silicon reached 90.56%, and the total leaching rate of iron reached 95.69%.

[0109] Those skilled in the art will appreciate that, without conflict, the above-mentioned preferred solutions can be freely combined and superimposed.

[0110] It should be understood that the above-mentioned embodiments are merely illustrative and not restrictive. Without departing from the basic principles of the present invention, various obvious or equivalent modifications or substitutions that can be made by those skilled in the art to the above-mentioned details will all be included in the scope of the claims of the present invention.

Claims

1. A method for comprehensive utilization of zinc concentrate roasted sand, wherein the zinc concentrate roasted sand comprises major elements zinc, silicon, iron and minor elements lead and silver, and the content of zinc is greater than that of iron, and the content of iron is greater than that of silicon; characterized in that: Includes steps: S10: mixing the zinc concentrate roasted sand with a sulfuric acid solution having an initial concentration of 100 g / L to 200 g / L, controlling the end point pH value of the solution to be 3 to 5, stirring at a temperature of 25° C. to 55° C. for 10 to 40 minutes, filtering and separating to obtain a first acid leaching solution and a first acid leaching residue; wherein the zinc element and the silicon element in the zinc concentrate roasted sand are leached into the first acid leaching solution, and the iron element, the lead element and the silver element remain in the first acid leaching residue; S20: continuing to react the first acid leaching solution at a temperature of 50° C. to 90° C., and then filtering and separating to obtain a second acid leaching solution and silica gel, wherein the zinc element in the first acid leaching solution is leached into the second acid leaching solution; S30: adding the first acid leaching residue to a sulfuric acid solution with an initial concentration of 200 g / L to 300 g / L, reacting for 1 to 3 hours, filtering and separating to obtain a third acid leaching solution and a second acid leaching residue; wherein the iron element in the first acid leaching residue is leached into the third acid leaching solution; and the lead element and the silver element remain in the second acid leaching residue; S40: adding the third acid leaching solution to a sulfuric acid solution with a pH value of 3 to 3.5, while controlling the pH value of the solution to be in the range of 3 to 3.5, so that the iron element in the third acid leaching solution is fully reacted to generate goethite, and filtering and separating to obtain a fourth acid leaching solution and goethite; S50: After adjusting the sulfuric acid concentration of the fourth acid leaching solution to the initial concentration of sulfuric acid in step 10, return to step S10.

2. The comprehensive utilization method of zinc concentrate roasted sand according to claim 1, characterized in that: In the step S10, the roasted zinc concentrate is added to a sulfuric acid solution with an initial concentration of 100 g / L to 200 g / L, stirred to mix the two, and the pH value of the solution at the end point is controlled to be 3 to 5 by controlling the amount of the roasted zinc concentrate added.

3. The comprehensive utilization method of zinc concentrate roasted sand according to claim 1, characterized in that: In the step S20, the first acid leaching solution is stirred at a temperature of 50°C to 90°C for 0.5 hour to 3 hours, and then filtered and separated.

4. The comprehensive utilization method of zinc concentrate roasted sand according to claim 1, characterized in that: The step S20 also includes the following steps: firstly treating the second acid leaching liquid through a purification step, and then electrolyzing and producing zinc.

5. The comprehensive utilization method of zinc concentrate roasted sand according to claim 1, characterized in that: In the step S30, the first acid leaching residue is added to the sulfuric acid solution at a temperature of 80°C to 110°C while stirring.

6. The comprehensive utilization method of zinc concentrate roasted sand according to claim 1, characterized in that: The first acid leaching residue also includes residual zinc element that has not been leached; In the step S30, the amount of the sulfuric acid solution is greater than the amount required to leach the iron and zinc in the first acid leaching residue, so that the iron and zinc elements in the first acid leaching residue are leached into the third acid leaching solution.

7. The comprehensive utilization method of zinc concentrate roasted sand according to claim 1, characterized in that: In the step S40, the pH value of the solution is controlled to be in the range of 3 to 3.5 by adding zinc oxide.

8. The comprehensive utilization method of zinc concentrate roasted sand according to claim 7, characterized in that: In the step S40, the third acid leaching solution is slowly added to the sulfuric acid solution at a temperature of 75° C. to 95° C., and the pH value of the solution is controlled to be in the range of 3 to 3.5 by controlling the addition rate of the third acid leaching solution and the addition rate of zinc oxide.

9. The comprehensive utilization method of zinc concentrate roasted sand according to claim 8, characterized in that: In the step S40, after all the third acid leaching solution is added to the sulfuric acid solution, stirring is performed for 10 minutes to 20 minutes, and then filtering and separating is performed.

10. A comprehensive utilization system of zinc concentrate roasted sand, used for implementing the comprehensive utilization method of zinc concentrate roasted sand according to any one of claims 1 to 9; characterized in that: include: A mixed reaction device for acid leaching reaction in steps S10, S20, S30 and S40, and a filtration separation device for filtration separation in steps S10, S20, S30 and S40.