Preparation method of Ti3C2Tx reinforced ZK61 magnesium alloy with continuously adjustable yield strength
By constructing a layered heterostructure, the specific mixing and sintering process of Ti3C2Tx and ZK61 magnesium powder was used to solve the problem of insufficient strength and plasticity of magnesium alloy, significantly improving the yield strength and hardness of magnesium alloy, and achieving high yield strength magnesium with magnesium strength Alloy preparation.
Patent Information
- Application Number
- CN202410864007.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-11-08
AI Technical Summary
Magnesium alloy materials have limited their application in the engineering field due to their low strength and poor plasticity. The prior art has limited effect in improving its mechanical properties.
By constructing a layered heterostructure, the two-dimensional material Ti3C2Tx is mixed with ZK61 magnesium powder, the distribution position of Ti3C2Tx is adjusted, and a discharge plasma sintering process with fast dense molding is used to prepare a Ti3C2Tx enhanced ZK61 magnesium alloy with high yield strength.
The elastic modulus, yield strength and hardness of Ti3C2Tx-5/ZK61 magnesium alloy samples were achieved, with an increase of 15.4%, 9.8%, and 12.3%, respectively, and a high yield strength that is continuously adjustable is high.
Smart Images

Figure CN118910448A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of enhancing the mechanical properties of ZK61 magnesium alloy by constructing a layered heterogeneous structure, and particularly relates to a preparation method thereof and application of a magnesium alloy with high yield strength. Background Art
[0002] Magnesium alloy is one of the lightest metal structural materials currently in practical application. It has high specific strength, high specific stiffness, excellent damping performance and electromagnetic shielding performance, and good biocompatibility. It is called "the green engineering material of the 21st century". With the advancement of science and technology, magnesium alloys are not only widely used in aerospace and automobile manufacturing fields, but also have important potential and application value in electronic devices, household appliances and medical surgery. However, the application of magnesium alloy materials in the engineering field has been inhibited due to their low strength and poor plasticity. In recent years, ceramic particles, carbon nanotubes, graphene, etc. have been added to magnesium alloys as reinforcements, and the strength or plasticity of their mechanical properties has been improved to varying degrees, which provides the possibility for the industrialization of high-strength and plastic magnesium alloys. Ti3C2T x As an emerging "graphene-like" two-dimensional material, it has mechanical properties, electrical conductivity, optical and electrochemical properties. At the same time, it has good metallic properties and dispersibility in aqueous solutions. Compared with other two-dimensional materials, the single layer has a high Young's modulus of 0.33±0.03TPa. The functional groups on the surface provide opportunities for its good dispersibility and excellent bonding in alloys. Studies have shown that heterostructure materials can effectively improve the relevant properties of metal materials. On this basis, the present invention constructs a layered heterostructure and obtains high yield strength Ti3C2T through a rapid dense molding spark plasma sintering process. x Strengthening ZK61 magnesium alloy provides a new path for the further development of magnesium alloys with high yield strength.
[0003] Ti3C2T with layered heterostructure x The preparation process of enhanced ZK61 magnesium alloy is mainly through adjusting Ti3C2T x Distribution position in ZK61 powder. x The hardness and compression properties of the reinforced ZK61 magnesium alloy samples were tested to obtain Ti3C2T with high yield strength. x Strengthened ZK61 alloy provides the basis. Summary of the invention
[0004] The purpose of the present invention is to transform the two-dimensional material Ti3C2T x Mixed with ball-milled ZK61 magnesium powder, the mixed Ti3C2T xThe ZK61 powder was pressed into tablets, and the flake powder blocks were arranged in a specific manner to construct a layered heterogeneous structure. The powder blocks were then sintered to prepare test samples. x The hardness and compression properties of the enhanced ZK61 alloy samples were tested in batches, and Ti3C2T with continuously adjustable high yield strength was obtained. x Enhanced ZK61 sample.
[0005] By adjusting Ti3C2T x Enhance the arrangement of ZK61 powder flakes and sinter them into a layer of Ti3C2T x Ti3C2T x -1 / ZK61, containing 2 layers of Ti3C2T x Ti3C2T x -2 / ZK61, containing 3 layers of Ti3C2T x Ti3C2T x -3 / ZK61, containing 5 layers of Ti3C2T x Ti3C2T x -5 / ZK61 sample. x The reinforced ZK61 magnesium alloy samples were subjected to compression tests and the Ti3C2T x -5 / ZK61 magnesium alloy sample has an elastic modulus of 60.8MPa, a yield strength of 210.7MPa, and a hardness of 78.3HV, which are increased by 15.4%, 9.8%, and 12.3% respectively. To achieve the above purpose, the technical solution adopted by the present invention is:
[0006] A Ti3C2T3 with continuously adjustable yield strength x The method for preparing enhanced ZK61 comprises the following steps:
[0007] (1) The ZK61 powder was ball-milled with a ball-to-powder ratio of 10:1, a ball-milling time of 1 h, and a rotation speed of 400 rpm;
[0008] (2) Add Ti3C2T x Solution, ZK61 powder and Ti3C2T x Mixing at a mass ratio of 20:1 to obtain a mixed solution;
[0009] (3) The mixed solution in (2) was allowed to stand for a period of time, and then the supernatant was removed and vacuum dried to obtain Ti3C2T x Mixed powder with ZK61;
[0010] (4) Weigh a certain amount of the mixed powder 5 times and pre-press it into tablets;
[0011] (5) The flaky mixed powders were loaded into a sintering mold in a certain order and subjected to spark plasma sintering. The axial pressure was 50 MPa and the temperature was kept at 500 °C for 5 min to obtain a gradient Ti3C2T with high yield strength. x Reinforced ZK61 magnesium alloy.
[0012] Furthermore, in step (1), the purpose of using a ball-to-material ratio of 10:1 and a rotation speed of 400 r / min is to remove the oxide layer on the surface of ZK61 to prevent the oxide layer from interfering with the ZK61 and Ti3C2T x The combination between.
[0013] Furthermore, the mass of each mixed powder piece in (3) is 0.6 g.
[0014] Furthermore, the arrangement in (4) is carried out in a certain order to achieve a layered arrangement.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The method of the present invention changes Ti3C2T x The arrangement in ZK61 constructs a specific layered heterostructure and obtains Ti3C2T with continuously adjustable high yield strength. x Enhanced ZK61 sample.
[0017] 2. Preparation of Ti3C2T by the present invention x -1 / ZK61, Ti3C2T x -2 / ZK61, Ti3C2T x -3 / ZK61, Ti3C2T x -5 / ZK61 magnesium alloy sample, after compression test, the Ti3C2T x -5 / ZK61 has greatly improved the elastic modulus, yield strength and hardness of magnesium alloy to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the preparation process of the present invention;
[0019] Figure 2 The Ti3C2T x -1 / ZK61, Ti3C2T x -2 / ZK61, Ti3C2T x -3 / ZK61, Ti3C2T x -5 / ZK61 sample and structural diagram;
[0020] Figure 3 The Ti3C2T x -1 / ZK61, Ti3C2Tx -2 / ZK61, Ti3C2T x -3 / ZK61, Ti3C2T x -5 / ZK61 sample optical microscope photo;
[0021] Figure 4 The Ti3C2T x -1 / ZK61, Ti3C2T x -2 / ZK61, Ti3C2T x -3 / ZK61, Ti3C2T x -5 / ZK61 sample stress compression test curve.
[0022] In the figure: 1. Dry Ti3C2T x and ZK61 magnesium alloy powder, 2. compacted ZK61 powder sheets, 3. compacted mixed powder sheets, 4. pulse current, 5. pressurization setting, 6. pressure punch, 7. mold, 8. mold cavity, 9. control system, 10. sample molding. DETAILED DESCRIPTION
[0023] The technical solution and effects of the present invention are further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.
[0024] The present invention adjusts Ti3C2T x Arrangement in ZK61 magnesium alloy, obtained with 1 layer of Ti3C2T x Ti3C2T x -1 / ZK61, containing 2 layers of Ti3C2T x Ti3C2T x -2 / ZK61, containing 3 layers of Ti3C2T x Ti3C2T x -3 / ZK61, containing 5 layers of Ti3C2T x Ti3C2T x -5 / ZK61.
[0025] Example 1
[0026] Weigh 20g of ZK61 powder and 200g of zirconium balls, pour the weighed powder into the ball mill, and after the ball mill is sealed, use a vacuum pump to extract the excess air in the jar, and then introduce argon into the jar. Set the ball milling process parameters to a speed of 400r / min and a ball milling time of 1h. Measure Ti3C2T with a concentration of 4.33mg / mL. xThe solution was poured into a beaker containing 300 mL of deionized water, and the ball-milled ZK61 powder was mixed with the mixture. The precipitate in the solution was collected in a petri dish and vacuum dried. The original powder and the dried mixed powder were weighed in batches of 0.6 g for 5 times, of which the mixed powder was weighed once. The weighed powders were pre-compacted, and 5 pieces of powder were placed in a sintering mold and sintered to obtain Ti3C2T x -1 / ZK61 magnesium alloy sample.
[0027] The Ti3C2T x -1 / ZK61 sample and structure diagram Figure 2 (a, b) shows; Ti3C2T in this embodiment x -1 / ZK61 Optical microscope photos Figure 3 (a) shows; Ti3C2T in this embodiment x -1 / ZK61 compression test is performed by Figure 4 As shown;
[0028] Example 2
[0029] Weigh 20g of ZK61 powder and 200g of zirconium balls, pour the weighed powder into the ball mill, and after the ball mill is sealed, use a vacuum pump to extract the excess air in the jar, and then introduce argon into the jar. Set the ball milling process parameters to a speed of 400r / min and a ball milling time of 1h. Measure Ti3C2T with a concentration of 4.33mg / mL. x The solution was poured into a beaker containing 300 mL of deionized water, and the ball-milled ZK61 powder was mixed with the mixture. The precipitate in the solution was collected in a petri dish and vacuum dried. The original powder and the dried mixed powder were weighed in batches of 0.6 g for 5 times, of which the mixed powder was weighed twice. The weighed powders were pre-compacted, and 5 pieces of powder were placed in a sintering mold and sintered to obtain Ti3C2T x -2 / ZK61 magnesium alloy samples.
[0030] The Ti3C2T x -2 / ZK61 sample and structure diagram Figure 2 (c, d); Ti3C2T in this embodiment x -2 / ZK61 optical microscope photos Figure 3 (b) As shown; in this embodiment, Ti3C2T x -2 / ZK61 compression test is performed by Figure 4 As shown;
[0031] Example 3
[0032] Weigh 20g of ZK61 powder and 200g of zirconium balls, pour the weighed powder into the ball mill, and after the ball mill is sealed, use a vacuum pump to extract the excess air in the jar, and then introduce argon into the jar. Set the ball milling process parameters to a speed of 400r / min and a ball milling time of 1h. Measure Ti3C2T with a concentration of 4.33mg / mL. x The solution was poured into a beaker containing 300 mL of deionized water, and the ball-milled ZK61 powder was mixed with the mixture. The precipitate in the solution was collected in a petri dish and vacuum dried. The original powder and the dried mixed powder were weighed in batches of 0.6 g for 5 times, of which the mixed powder was weighed 3 times. The weighed powders were pre-compacted, and 5 pieces of powder were placed in a sintering mold and sintered to obtain Ti3C2T x -3 / ZK61 magnesium alloy samples.
[0033] The Ti3C2T x -3 / ZK61 sample and structure diagram Figure 2 (e, f) shows; Ti3C2T in this embodiment x -3 / ZK61 optical microscope photos Figure 3 (c) shows; Ti3C2T in this embodiment x -3 / ZK61 compression test is performed by Figure 4 As shown;
[0034] Example 4
[0035] Weigh 20g of ZK61 powder and 200g of zirconium balls, pour the weighed powder into the ball mill, and after the ball mill is sealed, use a vacuum pump to extract the excess air in the jar, and then introduce argon into the jar. Set the ball milling process parameters to a speed of 400r / min and a ball milling time of 1h. Measure Ti3C2T with a concentration of 4.33mg / mL. x The solution was poured into a beaker containing 300 mL of deionized water, and the ball-milled ZK61 powder was mixed with the mixture. The precipitate in the solution was collected in a petri dish and vacuum dried. The original powder and the dried mixed powder were weighed in batches of 0.6 g for 5 times, of which the mixed powder was weighed 5 times. The weighed powders were pre-compacted, and 5 pieces of powder were placed in a sintering mold and sintered to obtain Ti3C2T x -5 / ZK61 magnesium alloy samples.
[0036] The Ti3C2T x -5 / ZK61 sample and structure diagram Figure 2 (g, h); Ti3C2T in this embodimentx -5 / ZK61 Optical microscope photos Figure 3 (d) shows; Ti3C2T in this embodiment x -5 / ZK61 compression test is performed by Figure 4 As shown;
[0037] Compression test experiment, Ti3C2T x -1 / ZK61, Ti3C2T x -2 / ZK61, Ti3C2T x -3 / ZK61, Ti3C2T x -5 / ZK61 magnesium alloy properties, specific results are shown in Table 1.
[0038] Table 1 ZK61, Ti3C2T x -1 / ZK61, Ti3C2T x -2 / ZK61, Ti3C2T x -3 / ZK61, Ti3C2T x -5 / ZK61 magnesium alloy compression properties
[0039]
[0040] It can be seen from Table 1 that the present invention and Ti3C2T x -1 / Zk61 compared to Ti3C2T x -5 / ZK61 magnesium alloy sample has an elastic modulus of 6.0 GPa, a yield strength of 210.7 MPa, and a hardness of 78.3 HV, which are increased by 15.4%, 9.8%, and 12.3%, respectively. This indicates that by changing the Ti3C2T x The distribution in ZK61 magnesium alloy can improve the yield strength of magnesium alloy to a certain extent and has continuous adjustability.
[0041] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A Ti with continuously adjustable yield strength 3 C 2 T x Preparation method of reinforced ZK61 magnesium alloy, It is characterized in that The preparation method comprises the following steps: (1) The ZK61 powder was ball-milled with a ball-to-powder ratio of 10:1, a ball-milling time of 1 h, and a rotation speed of 400 rpm; (2) Add Ti to the ball-milled ZK61 powder 3 C 2 T x Solution, ZK61 powder and Ti 3 C 2 T x Mixing at a mass ratio of 20:1 to obtain a mixed solution; (3) Let the mixed solution in (2) stand for a while, then remove the supernatant and vacuum dry to obtain Ti 3 C 2 T x Enhanced ZK61 mixed powder; (4) Weigh a certain amount of the mixed powder 5 times and pre-press it into tablets; (5) The mixed powder in flake form is loaded into a sintering mold in a certain order and spark plasma sintered at an axial pressure of 50 MPa and maintained at 500°C for 5 min to obtain Ti with high yield strength. 3 C 2 T x Reinforced ZK61 magnesium alloy.
2. The layered heterostructured Ti according to claim 1 3 C 2 T x Preparation method of reinforced ZK61 magnesium alloy, It is characterized in that In the preparation method, Ti 3 C 2 T x The mass ratio of ZK61 magnesium alloy powder is 0.005:
1.
3. The layered heterostructured Ti according to claim 1 3 C 2 T x Preparation method of reinforced ZK61 magnesium alloy, It is characterized in that The mass of each mixed powder piece in (4) is 0.6 g.
4. The Ti with continuously adjustable yield strength according to claim 1 3 C 2 T x Preparation method of reinforced ZK61 magnesium alloy, It is characterized in that The above (5) is arranged in a certain order to construct a specific layered heterostructure to obtain Ti with continuously adjustable yield strength. 3 C 2 T x Reinforced ZK61 magnesium alloy.