High-conductivity beryllium copper foil material for VCM elastic sheet and preparation method of high-conductivity beryllium copper foil material

By adding beryllium, cobalt, nickel and rare earth elements to the copper alloy and using detailed heat treatment and rolling processes, a high-conductivity beryllium copper foil was prepared, which solved the problem of difficulty in balance of strength and toughness of extremely thin beryllium copper foils. , improves the mechanical and conductive properties of VCM shrapnel, reduces energy consumption and extends the service life of the equipment.

CN118910463AInactive Publication Date: 2024-11-08国工恒昌新材料(义乌)有限公司

Patent Information

Application Number
CN202411408883.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing beryllium copper foils have difficulty balancing strength and toughness under extremely thin thicknesses, especially the mechanical properties under complex stresses, which affect the stability and durability of VCM shrapnel.

Method used

By adding appropriate amounts of beryllium, cobalt, nickel and rare earth elements to the copper alloy, combined with detailed heat treatment and rolling processes, beryllium copper foil with high conductivity, tensile strength and yield strength was prepared, with the thickness controlled at 0.045mm -0.08mm.

Benefits of technology

It improves the strength, hardness and conductivity of the material, reduces current transmission losses, improves the driving force and response speed of the VCM motor, reduces energy consumption and heat generation, and extends the equipment life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910463A_ABST
    Figure CN118910463A_ABST
Patent Text Reader

Abstract

The invention discloses a high-conductivity beryllium copper foil material for a VCM elastic sheet and a preparation method of the high-conductivity beryllium copper foil material, and relates to the field of beryllium copper foil material preparation. 0.35% to 0.6% of Co; 0.1% to 0.3% of Re; ni + Co is greater than 0.2%; and the balance of Cu. A proper amount of beryllium, cobalt, nickel and rare earth elements are added into the copper alloy, so that the strength, hardness and conductivity of the alloy are improved, and the alloy has a good age hardening effect, can well meet the requirements for manufacturing VCM elastic pieces and is a novel alloy material with excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention mainly relates to the technical field of beryllium copper foil preparation, and specifically relates to a high-conductivity beryllium copper foil for VCM shrapnel and a preparation method thereof. Background Art

[0002] VCM motor, or voice coil motor, is a linear DC motor that has become the mainstream choice for mobile terminal cameras due to its compact size and simple structural design. It generates electromagnetic thrust in a permanent magnetic field through an energized coil, and interacts with the deformation reaction force of the front and rear springs to form a combined force to drive the lens group to move forward and backward, achieving precise focus and ensuring clear images.

[0003] The material used for VCM springs needs to comprehensively consider the requirements of elasticity, mechanical properties, processing performance, environmental protection and cost-effectiveness. Among them, the strength and hardness of the material are to withstand various forces and torques when the motor is working, ensuring the stability and durability of the spring; the conductivity of the material is to improve the driving efficiency, reduce energy consumption and heat generation; Beryllium copper foil is a commonly used material for VCM springs; In the existing technology for the production and preparation of beryllium copper foil, as the thickness of the beryllium copper foil decreases, the balance between the strength and toughness of the beryllium copper foil will change; although the beryllium copper alloy itself has high strength and hardness, its ability to resist external mechanical stress may decrease at extremely thin thickness, especially when it needs to withstand complex stresses such as bending and twisting, which increases the difficulty of production and processing. Summary of the invention

[0004] Based on this, the object of the present invention is to provide a high conductivity beryllium copper foil for VCM shrapnel and a preparation method thereof, so as to solve the technical problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions: A high conductivity beryllium copper foil for VCM shrapnel, comprising the following components by mass percentage: Be: 0.15%-0.5%; Co: 0.35%-0.6%; Re: 0.1%-0.3%; Ni+Co>0.2%; The balance is Cu.

[0006] Preferably, the beryllium copper foil has a conductivity of ≥50%, a tensile strength of ≥850 MPa, a yield strength of ≥800 MPa, an elongation of ≥17%, a stress relaxation of ≤5% at a temperature of 100°C, and a thickness of 0.045 mm-0.08 mm.

[0007] A method for preparing a high-conductivity beryllium copper foil for a VCM shrapnel is also provided, which is applied to the high-conductivity beryllium copper foil for a VCM shrapnel, and comprises the following steps: S1: The raw materials are melted in a vacuum degassing melting furnace, and then an ingot is obtained by semi-continuous casting; S2: Electroslag remelting, forging, cutting off the head and tail of the ingot, and hot rolling the ingot to initially obtain thick alloy coils; S3: performing a first solution heat treatment, four-side milling, rough rolling, rough trimming, and a second solution heat treatment on the obtained thick alloy coil to obtain a thicker alloy coil; S4: the thicker alloy coil is subjected to a first cleaning and grinding, intermediate / finishing rolling, a third solution heat treatment, a second cleaning and grinding, and a second finishing rolling to a finished product thickness; S5: The finished product is cleaned and degreased, subjected to aging heat treatment, cleaned again, bent and straightened, and cut into pieces to obtain the final beryllium copper foil.

[0008] Preferably, in S1, the casting temperature is 1300-1500°C, the casting process adopts the pull-stop process, the pulling speed is 40-65m / min, the crystallizer vibration frequency is 30-50 times / min, the crystallizer amplitude is 3-5mm, and the casting size is 350x580x (670-1000) ingot.

[0009] Preferably, in S2, the electroslag remelting heat treatment process uses an electroslag remelting furnace at a temperature of 950-1050° C., and carbon powder is added to remove oxygen; The forging blank adopts three-fire forging, and the furnace heating process adopts 880℃x10h. After the first fire forging, it is not turned around for forging, but directly returned to the furnace for heating, and the heating process is 880℃x2h; the second fire is directly turned around forging, and the blank is punched out and then returned to the furnace, and the heating process is 880℃x2h; the third fire is directly punched out into the finished product size, and the finished product size is (75~105)x450x(3600~3800); The hot rolling blanking process is to heat the ingot to 880°C in a walking-beam heating furnace and keep it warm for 4-5 hours. The thickness of the ingot sheet is rolled from 100mm to 12mm, in the order of 100mm→85mm→67mm→53mm→41mm→31mm→24mm→19mm→15mm→12mm; the thickness of the thick alloy coil is 12mm.

[0010] Preferably, in S3, the process of the first solution heat treatment is: heating the hot-rolled thick alloy coil to 830-850° C. in a box-type heating furnace and keeping the temperature for 2-4 hours; The four-side milling process is as follows: the thick alloy coil after solution is put on a milling machine for uncoiling, straightening, side milling, upper and lower surface milling, and re-coiling. The thick alloy coil is milled for the first time, with each upper and lower milling surface of 0.5-0.6 mm and each side milling surface of 5 mm.

[0011] Preferably, in S3, the rough rolling process is as follows: the thick alloy plate after milling is rolled from 12mm to 1.2mm by a four-roll rough rolling mill, in the order of 12mm→11.2mm→9.9mm→8.8mm→6.8mm→5.9mm→4.6mm→4.0mm→3.1mm→2.5mm→1.8mm→1.2mm, with a total of 11 rolling passes, an actual rolling force of 300-420t, a rolling speed controlled at 35-55m / min, front and rear tensions controlled at 20~45KN, positive bending rolls are adopted during rolling, and the bending roll force is set to +6t; The rough cutting process size is: 5~10mm; the second solution heat treatment process is: air cushion continuous annealing furnace, annealing temperature is 820~850℃, annealing speed is 44~46m / min; the thickness of the thicker alloy coil is 1.2mm.

[0012] Preferably, in S4, the first cleaning and grinding process uses a thin belt cleaning machine, the grinding brush is made of SiC material, the mesh size is: 3000 mesh, and the grinding current is 7~9A; The medium / finishing rolling process uses a four-roll medium rolling mill to roll the plate to 0.103mm, in the order of 1.2mm→0.9mm→0.7mm→0.55mm→0.43mm→0.33m→0.27mm→0.22mm→0.17mm→0.14mm→0.12mm→0.103mm, with a total of 11 rolling passes, a rolling speed of 120~180m / min, and the front and rear tensions controlled at 20~40KN.

[0013] Preferably, in S4, the third solution heat treatment process is: an air cushion continuous annealing furnace, an annealing temperature of 820-850° C., and an annealing speed of 51-54 / min; The second cleaning and grinding process adopts a thin belt sander for cleaning, the cleaning speed is 40-60m / min, and the grinding brush current is 0.8-1.2A; The second finishing rolling adopts a twenty-roll finishing mill to roll from 0.103mm to the target size thickness of the high conductivity beryllium copper foil finished product, with a total of 2 rolling passes, a rolling speed of 140-240m / min, a working roll roughness requirement of ≤0.12mm, and a front and rear tension control of 6-12KN.

[0014] Preferably, in S5, the aging heat treatment is carried out in a bell furnace, the aging temperature is 360-430° C., the heating time is 3-6 hours, and the holding time is 7-10 hours.

[0015] In summary, the present invention mainly has the following beneficial effects: The invention improves the strength, hardness and electrical conductivity of the alloy by adding appropriate amounts of beryllium, cobalt, nickel and rare earth elements into the copper alloy. The alloy has a good aging hardening effect, so it has high strength, hardness and elastic limit after heat treatment. In the preparation process of high-conductivity beryllium copper foil, a detailed preparation method is used, and a high-precision rolling mill is used to ensure that the thickness is between 0.045 mm and 0.08 mm, which can well meet the requirements of manufacturing VCM shrapnel. The invention is a new alloy material with excellent comprehensive performance. In the use of VCM motors, highly conductive spring materials can reduce the loss of current during transmission and improve the current transmission efficiency; this means that under the same voltage, springs made of highly conductive materials can carry a larger current, thereby generating a stronger driving force, which is crucial to improving the response speed and driving force of VCM motors. At the same time, materials with good conductivity produce less resistance when current passes through, thereby reducing heat loss due to resistance; this not only helps reduce the energy consumption of the VCM motor, but also helps reduce performance degradation and shortened life due to heat; this is especially important for VCM motors that need to run for long periods of time or work under high load conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The present invention is a process flow chart of the preparation of beryllium copper foil; Figure 2 This is a hot rolling process parameter diagram for the preparation of the 0.06 specification beryllium copper foil of the present invention; Figure 3 This is a diagram of process parameters for rough rolling and embryo opening in the preparation of 0.06 specification beryllium copper foil of the present invention; Figure 4 This is a diagram of the process parameters for the intermediate / finishing rolling of the 0.06 specification beryllium copper foil of the present invention; Figure 5 This is a diagram of the finishing rolling process parameters in the preparation of the 0.06 specification beryllium copper foil of the present invention. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Example

[0018] like Figures 1 to 5As shown, a high conductivity beryllium copper foil material for VCM shrapnel includes the following components by mass percentage: Be: 0.15%-0.5%; Co: 0.35%-0.6%; Re: 0.1%-0.3%; Ni+Co>0.2%; The remainder is Cu; The conductivity of beryllium copper foil is ≥50%, the tensile strength is ≥850MPa, the yield strength is ≥800MPa, the elongation is ≥17%, the stress relaxation at 100℃ is ≤5%, and the thickness is between 0.045mm-0.08mm; A method for preparing a high-conductivity beryllium copper foil for a VCM shrapnel is also provided, which is applied to the high-conductivity beryllium copper foil for a VCM shrapnel, and comprises the following steps: Step 1: Smelting the raw materials in a vacuum degassing melting furnace, and then obtaining an ingot by semi-continuous casting; Step 2: Electroslag remelting, forging, cutting off the head and tail of the ingot, and hot rolling the ingot to initially obtain a thick alloy coil; Step 3: The obtained thick alloy coil is subjected to a first solution heat treatment, four-side milling, rough rolling, rough edge cutting, and a second solution heat treatment to obtain a thicker alloy coil; Step 4: The thicker alloy coil is subjected to a first cleaning and grinding, intermediate / finishing rolling, a third solution heat treatment, a second cleaning and grinding, and a second finishing rolling to a finished product thickness; Step 5: The finished product is cleaned and degreased, subjected to aging heat treatment, cleaned again, bent and straightened, and cut into pieces to obtain the final beryllium copper foil; In step 1, the casting temperature is 1300-1500°C, the casting process adopts the pull-stop process, the pull casting speed is 40-65m / min, the crystallizer vibration frequency is 30-50 times / min, the crystallizer amplitude is 3-5mm, and the casting size is 350x580x (670-1000) ingot; In step 2, the electroslag remelting heat treatment process uses an electroslag remelting furnace at a temperature of 950-1050°C, and carbon powder is added to remove oxygen; The forging process is three-fire forging, and the furnace heating process is 880℃x10h. After the first fire forging, it is directly returned to the furnace for heating without turning around, and the heating process is 880℃x2h; the second fire is directly turned around forging, and the blank is punched out and then returned to the furnace, and the heating process is 880℃x2h; the third fire is directly punched out into the finished product size, and the finished product size is (75~105)x450x(3600~3800); The hot rolling process is to heat the ingot to 880℃ in a walking beam heating furnace, keep it warm for 4-5h, and roll the ingot sheet from 100mm to 12mm in the following order: 100mm→85mm→67mm→53mm→41mm→31mm→24mm→19mm→15mm→12mm; the thickness of the thick alloy coil is 12mm; In step 3, the process of the first solution heat treatment is as follows: the thick alloy coil after hot rolling is heated to 830-850°C in a box-type heating furnace and kept at this temperature for 2-4 hours; The four-side milling process is as follows: the thick alloy coil after solution treatment is put on the milling machine for uncoiling - straightening - side milling - upper and lower surface milling - re-coiling. The thick alloy coil is milled for the first time, with the upper and lower milling surfaces of 0.5~0.6mm and the two side milling surfaces of 5mm each; In step 3, the rough rolling process is as follows: the thick alloy plate after milling is rolled from 12mm to 1.2mm by a four-roll rough rolling mill, in the order of 12mm→11.2mm→9.9mm→8.8mm→6.8mm→5.9mm→4.6mm→4.0mm→3.1mm→2.5mm→1.8mm→1.2mm, with a total of 11 passes, the actual rolling force is 300-420t, the rolling speed is controlled at 35-55m / min, the front and rear tensions are controlled at 20~45KN, and positive bending rolls are adopted during rolling, and the bending roll force is set to +6t; The rough cutting process size is: 5~10mm; the second solution heat treatment process is: air cushion continuous annealing furnace, annealing temperature is 820~850℃, annealing speed is 44~46m / min; the thickness of the thicker alloy coil is 1.2mm; In step 4, the first cleaning and grinding process uses a thin belt cleaning machine, the grinding brush is made of SiC material, the mesh size is: 3000 mesh, and the grinding current is 7~9A; The medium / finishing rolling process uses a four-roll medium rolling mill to roll the plate to 0.103mm, in the order of 1.2mm→0.9mm→0.7mm→0.55mm→0.43mm→0.33m→0.27mm→0.22mm→0.17mm→0.14mm→0.12mm→0.103mm, with a total of 11 passes, a rolling speed of 120~180m / min, and front and rear tensions controlled at 20~40KN; In step 4, the third solution heat treatment process is: air cushion continuous annealing furnace, annealing temperature is 820~850℃, annealing speed is 51~54 / min; The second cleaning and grinding process uses a thin belt sander for cleaning, with a cleaning speed of 40~60m / min and a grinding brush current of 0.8~1.2A; The second finishing rolling adopts a 20-roller finishing mill to roll from 0.103mm to the target thickness of the high conductivity beryllium copper foil finished product, with a total of 2 passes, a rolling speed of 140-240m / min, a working roll roughness requirement of ≤0.12mm, and a front and rear tension control of 6-12KN; In S5, the aging heat treatment is carried out in a bell furnace, the aging temperature is 360~430℃, the heating time is 3~6h, and the holding time is 7~10h.

[0019] Taking the preparation of high conductivity beryllium copper foil with a thickness of 0.06 mm as an example, it should be noted that in this embodiment; The beryllium copper alloy is placed in a smelting furnace and heated to a temperature above 1030°C to completely melt it. During the smelting process, cobalt, nickel and rare earth elements are added to adjust the properties of the material. The casting temperature is 1300-1500℃. The casting process adopts the pull-stop process. The billet pulling operation is carried out for a period of time. The casting speed is 40-65m / min, so that the molten metal gradually solidifies into a billet shell in the crystallizer. The crystallizer vibration frequency is 30-50 times / min, and the crystallizer amplitude is 3-5mm. Then the billet pulling is stopped to allow the melt to solidify in the crystallizer for more time, thereby thickening the billet shell and improving the tensile strength. An ingot with a size of 350x580x800 is obtained through casting; Then, the electroslag remelting heat treatment is carried out. In the electroslag remelting furnace, the temperature is maintained at 950~1050℃, the ingot is refined, and carbon powder is added to remove oxygen; so that it has better mechanical properties and corrosion resistance; In the forging process, the target finished product specifications are determined to be 100x450x3600; Three-fire forging is adopted. First, the ingot is charged into the furnace and heated at 880℃x10h. After the first fire forging, it is directly returned to the furnace for heating without turning around forging. The heating process is 880℃x2h. The second fire is directly turned around forging, and the blank is punched out and then returned to the furnace. The heating process is 880℃x2h. The third fire is directly punched out into the finished product specifications. Through forging, the defects of the beryllium copper alloy such as loose casting produced in the smelting process can be eliminated, and the microstructure can be optimized. Then the parts with cracks and pores at the head and tail are cut off and hot rolled to form a thick alloy coil with a thickness of 12mm. The hot rolling process is to heat the ingot to 880℃ in a walking beam heating furnace and keep it warm for 4~5h. The thickness of the ingot sheet is rolled from 100mm to 12mm, in the order of 100mm→85mm→67mm→53mm→41mm→31mm→24mm→19mm→15mm→12mm. The specific process parameters are as follows: Figure 2 As shown; Heat the 12mm thick alloy coil to 830~850℃ in a box-type heating furnace and keep it warm for 2-4h; and use oil quenching to improve the high-strength performance of the material; After the thick alloy coil is cooled, it is then milled on four sides. The process is as follows: the thick alloy coil is unrolled - straightened - milled on the side - milled on the upper and lower surfaces - re-rolled. The thick alloy coil is milled once, with each upper and lower milling surface of 0.5mm and each side milling surface of 5mm; Then the rough rolling is carried out, and the process is as follows: the thick alloy plate after milling is rolled from 11mm to 1.2mm by a four-roll rough rolling mill, in the order of 11mm→10.2mm→8.9mm→8.0mm→6.8mm→5.9mm→4.6mm→4.0mm→3.1mm→2.5mm→1.8mm→1.2mm, with a total of 11 passes, the actual rolling force is 300-420t, the rolling speed is controlled at 35-55m / min, the front and rear tensions are controlled at 20~45KN, and the positive bending roll is adopted during rolling, and the bending roll force is set to +6t; the specific process parameters are as follows Figure 3 Shown: Then, the rough cutting is performed and then the solution heat treatment is performed to obtain a thicker alloy coil with a thickness of 1.2 mm. In this embodiment, the crack depth of the coil edge is small, and the rough cutting edge size is 5 mm; During the second solution heat treatment, the process is: air cushion continuous annealing furnace, annealing temperature is 820~850℃, annealing speed is 44~46m / min; For thicker alloy coils, a thin belt cleaning machine is used for cleaning and grinding. The grinding brush is made of SiC, with a mesh size of 3000 and a grinding current of 7~9A. The loss in this grinding process is small, and the thickness loss is not counted. Then, a four-roller intermediate rolling mill is used for intermediate / finishing rolling. The target size is to roll the sheet to 0.10 mm, which is 1.2 mm → 0.9 mm → 0.7 mm → 0.55 mm → 0.43 mm → 0.33 mm → 0.27 mm → 0.22 mm → 0.17 mm → 0.14 mm → 0.12 mm → 0.10 mm in sequence. There are 11 passes in total. The rolling speed is 120-180 m / min, and the front and rear tensions are controlled at 20-40 KN. The specific process parameters are as follows: Figure 4 As shown: Then the third solution heat treatment is carried out, the process is: air cushion continuous annealing furnace, annealing temperature is 820~850℃, annealing speed is 51~54 / min; The second cleaning and grinding, the cleaning speed is 40~60m / min, the grinding brush current is 0.8~1.2A; After the secondary cleaning and grinding, the twenty-roller finishing mill is used for finishing rolling, from 0.1mm to 0.06mm, in the order of 0.10m→0.08mm→0.06mm, with a total of 2 passes, the rolling speed is 140~240m / min, the working roll roughness requirement is ≤0.12mm, and the front and rear tension is controlled at 6-12KN; the specific process parameters are as follows Figure 5 As shown: Finally, the finished product is cleaned and degreased, and aging heat treatment is carried out in a bell furnace, with an aging temperature of 360~430℃, a heating time of 3~6h, and a holding time of 7~10h; and the subsequent re-cleaning is completed, and the material is stretched, bent, straightened, and the finished product is cut to obtain a beryllium copper foil with a thickness of 0.06mm; The obtained beryllium copper foil has a conductivity of 90%, a tensile strength of 890 MPa, a yield strength of 828 MPa, an elongation of ≥17%, and a stress relaxation of ≤5% at a temperature of 100°C.

[0020] The above embodiments are only for illustrating the technical idea of ​​the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the present invention.

Claims

1. A high conductivity beryllium copper foil for VCM shrapnel, characterized in that , calculated by mass percentage, includes the following components: Be: 0.15%-0.5%; Co: 0.35%-0.6%; Re: 0.1%-0.3%; Ni+Co>0.2%; The balance is Cu.

2. The high conductivity beryllium copper foil for VCM shrapnel according to claim 1, characterized in that: The beryllium copper foil has a conductivity of ≥50%, a tensile strength of ≥850 MPa, a yield strength of ≥800 MPa, an elongation of ≥17%, a stress relaxation of ≤5% at a temperature of 100° C., and a thickness of 0.045 mm-0.08 mm.

3. A method for preparing a high-conductivity beryllium copper foil for a VCM shrapnel, applied to a high-conductivity beryllium copper foil for a VCM shrapnel as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: S1: The raw materials are melted in a vacuum degassing melting furnace, and then an ingot is obtained by semi-continuous casting; S2: Electroslag remelting, forging, cutting off the head and tail of the ingot, and hot rolling the ingot to initially obtain thick alloy coils; S3: performing a first solution heat treatment, four-side milling, rough rolling, rough trimming, and a second solution heat treatment on the obtained thick alloy coil to obtain a thicker alloy coil; S4: the thicker alloy coil is subjected to a first cleaning and grinding, intermediate / finishing rolling, a third solution heat treatment, a second cleaning and grinding, and a second finishing rolling to a finished product thickness; S5: The finished product is cleaned and degreased, subjected to aging heat treatment, cleaned again, bent and straightened, and cut into pieces to obtain the final beryllium copper foil.

4. The method for preparing a high-conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S1, the casting temperature is 1300-1500°C, the casting process adopts the pull-stop process, the pull speed is 40-65m / min, the crystallizer vibration frequency is 30-50 times / min, the crystallizer amplitude is 3-5mm, and the casting size is 350x580x (670-1000) ingot.

5. The method for preparing a high-conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S2, the electroslag remelting heat treatment process uses an electroslag remelting furnace with a temperature of 950-1050° C., and carbon powder is added to remove oxygen; The forging blank adopts three-fire forging, and the furnace heating process adopts 880℃x10h. After the first fire forging, it is not turned around for forging, but directly returned to the furnace for heating, and the heating process is 880℃x2h; the second fire is directly turned around forging, and the blank is punched out and then returned to the furnace, and the heating process is 880℃x2h; the third fire is directly punched out into the finished product size, and the finished product size is (75~105)x450x(3600~3800); The hot rolling blanking process is to heat the ingot to 880°C in a walking-beam heating furnace and keep it warm for 4-5 hours. The thickness of the ingot sheet is rolled from 100mm to 12mm, in the order of 100mm→85mm→67mm→53mm→41mm→31mm→24mm→19mm→15mm→12mm; the thickness of the thick alloy coil is 12mm.

6. The method for preparing a high conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S3, the process of the first solution heat treatment is: heating the hot-rolled thick alloy coil to 830-850° C. in a box-type heating furnace and keeping the temperature for 2-4 hours; The four-side milling process is as follows: the thick alloy coil after solution is put on a milling machine for uncoiling, straightening, side milling, upper and lower surface milling, and recoiling. The thick alloy coil is milled for the first time, with each upper and lower milling surface of 0.5-0.6 mm and each side milling surface of 5 mm.

7. The method for preparing a high conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S3, the rough rolling process is as follows: the thick alloy plate after milling is rolled from 12mm to 1.2mm by a four-roll rough rolling mill, in the order of 12mm→11.2mm→9.9mm→8.8mm→6.8mm→5.9mm→4.6mm→4.0mm→3.1mm→2.5mm→1.8mm→1.2mm, with a total of 11 rolling passes, an actual rolling force of 300-420t, a rolling speed controlled at 35-55m / min, front and rear tensions controlled at 20-45KN, positive bending rolls are adopted during rolling, and the bending roll force is set to +6t; The rough cutting process size is: 5~10mm; the second solution heat treatment process is: air cushion continuous annealing furnace, annealing temperature is 820~850℃, annealing speed is 44~46m / min; the thickness of the thicker alloy coil is 1.2mm.

8. The method for preparing a high-conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S4, the first cleaning and grinding process uses a thin belt cleaning machine, the grinding brush is made of SiC material, the mesh size is: 3000 mesh, and the grinding current is 7~9A; The medium / finishing rolling process uses a four-roll medium rolling mill to roll the plate to 0.103mm, in the order of 1.2mm→0.9mm→0.7mm→0.55mm→0.43mm→0.33m→0.27mm→0.22mm→0.17mm→0.14mm→0.12mm→0.103mm, with a total of 11 rolling passes, a rolling speed of 120~180m / min, and the front and rear tensions controlled at 20~40KN.

9. The method for preparing a high-conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S4, the third solution heat treatment process is: air cushion continuous annealing furnace, annealing temperature is 820-850° C., annealing speed is 51-54 / min; The second cleaning and grinding process adopts a thin belt sander for cleaning, the cleaning speed is 40-60m / min, and the grinding brush current is 0.8-1.2A; The second finishing rolling adopts a twenty-roll finishing mill to roll from 0.103mm to the target size thickness of the high conductivity beryllium copper foil finished product, with a total of 2 rolling passes, a rolling speed of 140-240m / min, a working roll roughness requirement of ≤0.12mm, and a front and rear tension control of 6-12KN.

10. The method for preparing a high conductivity beryllium copper foil for VCM shrapnel according to claim 3, characterized in that: In S5, the aging heat treatment is carried out in a bell furnace, the aging temperature is 360-430° C., the heating time is 3-6 hours, and the holding time is 7-10 hours.

Citation Information

Patent Citations

  • Copper alloy for manufacturing mould and preparation method thereof

    CN101705389A

  • Novel high-elasticity low beryllium copper alloy and preparation method thereof

    CN102719699A

  • High-strength and high softening temperature low beryllium-copper alloy and preparation method thereof

    CN108315581A

  • High-strength conductive copper alloy and preparation method thereof

    CN115976364A

  • Copper alloy foil for 5G mobile phone card slot and preparation method of copper alloy foil

    CN118222876A

Cited By

  • High-strength corrosion-resistant copper beryllium alloy sheet and preparation process thereof

    CN119144870A

  • Long-acting stress-resistant titanium-copper foil material for VCM elastic sheet and preparation method of long-acting stress-resistant titanium-copper foil material

    CN119456677A