High-conductivity and high-strength aluminum alloy wire and preparation method thereof

By controlling the casting and aging process, we ensure that the reinforced phase is analyzed for alloy element charging, which solves the problem that the conductivity and strength of aluminum alloy wires are difficult to increase at the same time, and achieves high conductivity and high strength aluminum alloy wires, which meet the safety of extreme climate conditions Requirements and simplification of production processes.

CN118910474APending Publication Date: 2024-11-08SHANGHAI JIAOTONG UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410209350.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing aluminum-magnesium silicon alloy wires are difficult to increase the conductivity and elongation at the same time after increasing the strength, and the production cost is high, resulting in the conductors being easily broken under extreme climate conditions, making it difficult to meet the requirements of high conductivity and high strength.

Method used

By controlling the temperature of continuous casting and extrusion and the temperature and time of rod material and monofilament aging, we ensure that the alloy element is filled and analyzed to analyze the β" and β' diffuse phases, and improve the conductivity and strength of the aluminum alloy wires, and directly form the rod using continuous casting and extrusion equipment. The material is subjected to dual aging treatment to simplify the production process.

Benefits of technology

Aluminum alloy wire with high conductivity and high strength is achieved, with a single wire strength of ≥315MPa, a conductivity of ≥57% IACS, and an elongation of ≥5%, while reducing production costs and improving production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a high-conductivity high-strength aluminum alloy wire and a preparation method thereof.The high-conductivity high-strength aluminum alloy wire comprises, by weight, 0.43%-0.52% of Mg, 0.44%-0.5% of Si, 0.12%-0.15% of Fe, 0.18%-0.3% of Y, 0.03%-0.05% of La, 0.005%-0.02% of B and the balance Al and other impurity elements, it is guaranteed that the temperature of a melt is kept within a proper range in the continuous casting and extruding process by controlling the temperature of continuous casting and extruding, and the high-conductivity high-strength aluminum alloy wire is obtained. On the other hand, by controlling the temperature and time of rod material aging and monofilament aging, it is ensured that the alloy elements are fully precipitated in a beta ''and beta 'dispersed phase mode, and the electric conductivity of the aluminum alloy wire is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aluminum alloy wires, and in particular to an aluminum alloy wire with high conductivity and high strength and a preparation method thereof. Background Art

[0002] Overhead transmission lines are the energy arteries of economic development. In some areas, extreme climates such as low temperature, rain, snow and freezing often occur. The conductors are prone to breakage and collapse due to ice. Therefore, high-breaking-force conductors must be used in ice-covered areas to ensure line safety. Overhead transmission projects in heavy ice areas generally use steel-core aluminum alloy stranded wires. At present, the strength of high-conductivity aluminum alloy wires with a conductivity of 57% IACS is mostly only 260-290MPa, and the conductor breaking force is insufficient; while the conductivity of high-strength aluminum alloy wires with a strength of 315MPa is only 52.5% IACS, which makes it difficult to achieve the green and low-carbon goals of energy conservation and emission reduction.

[0003] As we all know, the strength, elongation and conductivity of aluminum-magnesium-silicon alloy are mutually restricted. When the strength of the alloy is increased, the elongation and conductivity of the alloy will often decrease significantly. The current aluminum-magnesium-silicon alloy and conventional process routes are difficult to achieve a significant improvement in the comprehensive performance of the alloy wire, and face the problem of high production costs.

[0004] In the prior art, the manufacturing process of medium-strength aluminum-magnesium-silicon alloy wire is generally smelting, continuous casting and rolling, drawing, and aging treatment. On the one hand, the temperature of the continuous casting billet drops significantly during the rolling process, and a large amount of alloy elements precipitate, which cannot effectively exert their precipitation strengthening effect during aging. On the other hand, the precipitation process of aluminum-magnesium-silicon alloy under conventional aging technology is difficult to ensure that the alloy elements are fully precipitated in the form of β" and β' metastable strengthening phases, which limits the further improvement of the alloy performance. Summary of the invention

[0005] In view of the defects in the prior art, the purpose of the present invention is to provide an aluminum alloy wire with high conductivity and high strength and a preparation method thereof. By controlling the temperature of continuous casting and extrusion, the temperature of the melt is kept within a suitable range during the process to control the amount of alloy element precipitation. On the other hand, by controlling the temperature and time of rod aging and single wire aging, it is ensured that the alloy elements are fully precipitated in the form of β" and β' dispersed phases, thereby further improving the conductivity of the aluminum alloy wire.

[0006] A first aspect of the present invention provides an aluminum alloy wire with high conductivity and high strength. The aluminum alloy wire comprises the following components by weight percentage: Mg 0.43-0.52%, Si 0.44-0.5%, Fe 0.12-0.15%, Y 0.18-0.3%, La 0.03-0.05%, B 0.005-0.02%, and the balance is Al and other impurity elements.

[0007] In one embodiment, the weight percentages of the other impurity elements are: Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of the other impurity elements is ≤0.02%.

[0008] In one embodiment, the aluminum alloy wire has a single wire strength of ≥315 MPa, a conductivity of ≥57% IACS, and an elongation of ≥5%.

[0009] A second aspect of the present invention provides a method for preparing the above-mentioned high-conductivity and high-strength aluminum alloy wire, comprising the following steps:

[0010] S1, smelting, according to the element composition and weight percentage of the aluminum alloy wire, adding aluminum ingots, iron agent, silicon agent and aluminum rare earth alloy into a smelting furnace, heating and melting, then adding magnesium ingots, and fully stirring to obtain a first melt;

[0011] S2, refining in a furnace, adding aluminum-boron alloy to the first melt for boronization treatment, stirring thoroughly and then standing to cool, to obtain a second melt;

[0012] S3, online refining, performing online degassing and online filtering on the second melt to obtain a third melt;

[0013] S4, continuous casting and extrusion, wherein the third melt is cooled and solidified by continuous casting and extrusion equipment, and then extruded to obtain a first rod material;

[0014] S5, rod quenching, the first rod is subjected to online quenching cooling;

[0015] S6, rod aging, the rod material after online quenching is immediately subjected to rod aging treatment at 160-200°C, and kept at this temperature for 10-18 hours to obtain a second rod material;

[0016] S7, rod drawing, using a sliding wire drawing machine to draw the second rod after aging to obtain an aluminum alloy wire, wherein the diameter of the aluminum alloy wire is 2.5-4.0 mm;

[0017] S8, single wire aging, the aluminum alloy wire is subjected to single wire aging treatment at 150-180° C. and kept warm for 7-10 hours to obtain a refined aluminum alloy wire.

[0018] In one embodiment, in step S2, the stirring temperature of the furnace refining is 730-750°C, the stirring time of the furnace refining is 10-15 minutes, the standing temperature of the furnace refining is 720-730°C, and the standing time of the furnace refining is 25-40 minutes.

[0019] In one embodiment, in step S3, the online degassing uses a rotary spray degassing box, and the online filtration uses a double-stage foam ceramic filter box.

[0020] In one embodiment, the degassing medium of the rotary spray degassing box is high-purity nitrogen, the rotation speed of the graphite rotor is 400-500r / min; the porosity of the two-stage foam ceramic filter box is 30-50PPI.

[0021] In one embodiment, in step S4, the casting temperature of the continuous casting equipment is 690-710°C, the diameter of the first rod material is 9-10 mm, and the outlet temperature of the first rod material is 480-520°C.

[0022] In one embodiment, in step S7, the drawing speed of the sliding wire drawing machine is 10-15 m / s, and the sliding wire drawing machine adopts a nano-diamond composite coating mold.

[0023] In one embodiment, in steps S6 and S8, after rod aging, the first rod contains a first dispersed phase β" (Mg5Si6); after single wire aging, the first dispersed phase β" (Mg5Si6) and the second dispersed phase β' (Mg9Si5) are precipitated from the aluminum alloy wire.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. In the high-conductivity and high-strength aluminum alloy wire provided by the present invention, its constituent elements are designed, wherein Mg and Si elements can form a dispersion strengthening phase to improve strength, Fe and Si elements are beneficial to improving conductivity, and Y, La, and B elements can increase the number of crystal nuclei, refine the structure and improve the strength of the aluminum alloy wire.

[0026] 2. In the preparation method of the high-conductivity and high-strength aluminum alloy wire provided by the present invention, by controlling the temperature of the continuous casting and extrusion equipment and the temperature of the first rod material outlet, it is ensured that the process from the melt to the rod material is always in a high-temperature state, thereby solving the problem of premature precipitation of alloy elements from the rod material, thereby ensuring the supersaturated state of the alloy rod material, and providing sufficient conditions for the subsequent aging process.

[0027] 3. In the method for preparing the high-conductivity and high-strength aluminum alloy wire provided by the present invention, the quenched rod material is immediately subjected to aging treatment and the single wire is subjected to aging treatment. The double aging treatment can make the solid-solution alloy elements fully precipitate from the matrix in the form of dispersed phases β" (Mg5Si6) and β' (Mg9Si5), thereby improving the strength and conductivity of the aluminum alloy wire single wire.

[0028] 4. In the preparation method of the high-conductivity and high-strength aluminum alloy wire provided by the present invention, the continuous casting and extrusion equipment is used to directly extrude the melt into a rod material, which simplifies the production process and thus improves production efficiency; the extrusion process can also replace the number of dies at the extrusion outlet, increase or decrease them according to production needs, and flexibly adjust the production process. DETAILED DESCRIPTION

[0029] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0030] A first aspect of the present invention provides an aluminum alloy wire with high conductivity and high strength. The aluminum alloy wire comprises the following components by weight percentage: Mg 0.43-0.52%, Si 0.44-0.5%, Fe 0.12-0.15%, Y 0.18-0.3%, La 0.03-0.05%, B 0.005-0.02%, and the balance is Al and other impurity elements.

[0031] In some embodiments, the weight percentages of the other impurity elements are: Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of the other impurity elements is ≤0.02%.

[0032] In some embodiments, the aluminum alloy wire has a single wire strength of ≥315 MPa, a conductivity of ≥57% IACS, and an elongation of ≥5%.

[0033] A second aspect of the present invention provides a method for preparing the above-mentioned high-conductivity and high-strength aluminum alloy wire, comprising the following steps:

[0034] S1. Smelting: according to the element composition and weight percentage of the aluminum alloy wire, an aluminum ingot with a purity greater than 99.7%, an iron agent, a silicon agent and an aluminum rare earth alloy are added into a smelting furnace, heated to melt, and then a magnesium ingot is added, and a first melt is obtained after sufficient stirring;

[0035] S2, furnace refining, transferring the first melt in the smelting furnace to a tilting holding furnace, adding aluminum-boron alloy to the first melt for boronization treatment, stirring fully, adjusting the temperature of the first melt to 730-750° C., stirring time is 10-15 minutes, cleaning the scum on the surface of the first melt thoroughly and then standing to cool, the cooling temperature is 720-730° C., and the cooling standing time is 25-40 minutes to obtain a second melt;

[0036] S3, online refining, performing online degassing and online filtering on the second melt to obtain a third melt;

[0037] S4, continuous casting and extrusion, the third melt is poured into a rotating water-cooled groove wheel through a nozzle of a continuous casting and extrusion device, solidified in a cavity surrounded by a solidification shoe and a wheel groove, and then enters an extrusion shoe for extrusion and forming to obtain a first rod material;

[0038] S5, rod quenching, the first rod is quenched and cooled online with cooling water, the cooling water temperature is 20-30° C., and the extruded first rod is rolled after being quenched and cooled online;

[0039] S6, rod aging, the rod material after online quenching is immediately subjected to rod aging treatment at 160-200°C, and kept at this temperature for 10-18 hours to obtain a second rod material;

[0040] S7, rod drawing, using a sliding wire drawing machine to draw the second rod after aging to obtain an aluminum alloy wire, wherein the diameter of the aluminum alloy wire is 2.5-4.0 mm;

[0041] S8, single wire aging, the aluminum alloy wire is subjected to single wire aging treatment at 150-180° C. and kept warm for 7-10 hours to obtain a refined aluminum alloy wire.

[0042] In some embodiments, in step S3, the online degassing adopts a rotary jet degassing box, the degassing medium of the rotary jet degassing box is high-purity nitrogen, the rotation speed of the graphite rotor is 400-500r / min, and the online degassing makes the hydrogen content in the melt <0.12ml / 100g, which provides good raw materials for subsequent continuous casting and aging treatment, and further improves the subsequent production efficiency and product effect; the online filtration adopts a two-stage foam ceramic filter box, and the porosity of the two-stage foam ceramic filter box is 30-50PPI to remove 5-10μm inclusion particles in the third melt and reduce the adverse effects of inclusions on the elongation of the alloy single wire.

[0043] In some embodiments, in step S4, the casting temperature of the continuous casting equipment is 690-710°C, the diameter of the first rod is 9-10 mm, and the outlet temperature of the first rod is 480-520°C. The casting temperature and the outlet temperature of the first rod are kept in a relatively high range to ensure that the process from the melt to the rod is always in a high temperature state, thereby solving the problem of premature precipitation of alloy elements from the rod, thereby ensuring the supersaturated state of the alloy rod, and providing sufficient conditions for the subsequent aging process.

[0044] In some embodiments, in step S7, the drawing speed of the sliding wire drawing machine is 10-15m / s, and the precision of the rod drawing is controlled within ±0.01mm, which can ensure that the fineness of the final product meets the production standard; the sliding wire drawing machine uses a nano-diamond composite coating mold, which is a mold obtained by growing a layer of diamond film on the inner hole surface of the mold using a chemical vapor deposition method (CVD) with a cemented carbide (WC-Co) as a substrate, and precisely grinding and polishing the diamond coating, which can be obtained by commercial purchase. Since the strength of the second rod is relatively high after the rod aging of the present invention, the rod drawing process uses a nano-diamond composite coating mold, the coating surface of the mold is flat and smooth, and the friction coefficient is small, which can ensure the surface quality of the drawn single wire.

[0045] In some embodiments, in steps S6 and S8, the first rod material obtained by continuous casting and extrusion is immediately subjected to rod aging treatment after quenching, so that most of the Mg and Si elements are precipitated from the first rod material in the state of the first dispersed phase β" (Mg5Si6), while the natural aging process of the first rod material can be suppressed, avoiding the adverse effects of natural aging on the mechanical properties of the alloy wire, which is conducive to obtaining an alloy wire with higher strength; after single wire aging, the remaining alloy elements in solid solution are precipitated from the aluminum alloy wire in the form of the second dispersed phase β" (Mg5Si6), β' (Mg9Si5), further improving the conductivity and single wire strength.

[0046] The present invention is further described below in conjunction with embodiments:

[0047] Example 1

[0048] The present embodiment provides an aluminum alloy wire with high conductivity and high strength, which includes the following components by weight percentage: Mg 0.47%, Si 0.44%, Fe 0.15%, Y 0.25%, La 0.03%, B 0.008%, the balance is Al and unavoidable impurity elements, Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of impurity elements is ≤0.02%.

[0049] The preparation method of the high-conductivity and high-strength aluminum alloy wire in this embodiment is as follows:

[0050] S1. Smelting: according to the element composition and weight percentage of the aluminum alloy wire, an aluminum ingot with a purity greater than 99.7%, an iron agent, a silicon agent, and an aluminum rare earth alloy are added into a smelting furnace, heated to melt, and then a magnesium ingot is added and melted, and a first melt is obtained after sufficient stirring;

[0051] S2, furnace refining, the first melt is transferred to a tilting holding furnace, a trace amount of aluminum-boron alloy is added for boronization treatment, the tilting holding furnace is turned on for full stirring, the melt temperature in the furnace is adjusted to 740°C for furnace refining for 15 minutes, and then the slag on the surface of the melt is thoroughly scraped off to obtain a second melt, the temperature of the second melt is adjusted to 720°C, and the melt is allowed to stand for 30 minutes;

[0052] S3, online refining, online degassing and online filtering of the second melt to obtain a third melt, wherein the online degassing adopts a rotary spray degassing box with high-purity nitrogen as the degassing medium, the speed of the graphite rotor is 450r / min, and the hydrogen content in the melt is made less than 0.12ml / 100g by online degassing; the online filtration adopts a two-stage foam ceramic filter box with a porosity of 30 / 50PPI to remove 5-10μm inclusion particles in the melt and reduce the adverse effect of inclusions on the elongation of the alloy single wire;

[0053] S4, continuous casting and extrusion, pouring the third melt into the rotating water-cooled groove wheel through the nozzle of the continuous casting and extrusion equipment, solidifying and forming in the cavity surrounded by the solidification shoe and the wheel groove, and then entering the extrusion shoe for extrusion and forming to obtain the first rod material; wherein the casting temperature is 700°C, the cooling water temperature is 20°C, the extruded rod material diameter is 10mm, and the rod material temperature at the outlet is 490°C; the continuous casting and extrusion adopts the continuous casting and extrusion equipment conventionally used in the art, and the extrusion process adopts a three-outlet die, which can extrude three rod materials at the same time;

[0054] S5, rod quenching, using online cooling water to quench the first rod online, the water temperature is 20°C, and the extruded rod is rolled after online quenching and cooling;

[0055] S6, rod aging, the first rod is immediately subjected to aging treatment after quenching, the aging temperature is 170°C, the holding time is 15h, and the second rod obtained after aging contains dispersed β" (Mg5Si6) phase;

[0056] S7, rod drawing, using a sliding wire drawing machine to draw the second rod, the sliding wire drawing machine uses a nano-diamond composite coating die, the drawing speed is 12m / s, the final drawing dimensional accuracy is controlled within ±0.01mm, and a single wire diameter of 3.5mm is obtained. Aluminum alloy wire;

[0057] S8, single wire aging, aging treatment is performed on the aluminum alloy wire formed by drawing the rod, the temperature of the single wire aging is 150°C, the holding time is 8 hours, and a refined aluminum alloy wire is obtained after the single wire aging; wherein the remaining alloy elements in the refined aluminum alloy wire are further precipitated to form a second dispersed phase mainly composed of β" (Mg5Si6) and β' (Mg9Si5).

[0058] For the refined aluminum alloy wire in this embodiment, its single wire strength is measured by E45.504 tensile testing machine and is ≥315MPa; its conductivity is measured by PC36C DC resistance meter and is ≥57%IACS; its elongation is measured by electronic extensometer Y50 and is ≥5%.

[0059] Example 2

[0060] The present embodiment provides an aluminum alloy wire with high conductivity and high strength, which includes the following components by weight percentage: Mg 0.43%, Si 0.45%, Fe 0.12%, Y 0.18%, La 0.05%, B 0.005%, the balance is Al and unavoidable impurity elements, Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of impurity elements is ≤0.02%.

[0061] The preparation method of the high-conductivity and high-strength aluminum alloy wire in this embodiment is as follows:

[0062] S1. Smelting: according to the element composition and weight percentage of the aluminum alloy wire, an aluminum ingot with a purity greater than 99.7%, an iron agent, a silicon agent, and an aluminum rare earth alloy are added into a smelting furnace, heated to melt, and then a magnesium ingot is added and melted, and a first melt is obtained after sufficient stirring;

[0063] S2, furnace refining, the first melt is transferred to a tilting holding furnace, a trace amount of aluminum-boron alloy is added for boronization treatment, the tilting holding furnace is turned on for sufficient stirring, the melt temperature in the furnace is adjusted to 750°C for furnace refining for 13 minutes, and then the scum on the surface of the melt is thoroughly scraped off to obtain a second melt, the temperature of the second melt is adjusted to 730°C, and the melt is allowed to stand for 30 minutes;

[0064] S3, online refining, online degassing and online filtering of the second melt to obtain a third melt, wherein the online degassing adopts a rotary spray degassing box with high-purity nitrogen as the degassing medium, the speed of the graphite rotor is 450r / min, and the hydrogen content in the melt is made less than 0.12ml / 100g by online degassing; the online filtration adopts a two-stage foam ceramic filter box with a porosity of 30 / 50PPI to remove 5-10μm inclusion particles in the melt and reduce the adverse effect of inclusions on the elongation of the alloy single wire;

[0065] S4, continuous casting and extrusion, pouring the third melt into the rotating water-cooled groove wheel through the nozzle of the continuous casting and extrusion equipment, solidifying and forming in the cavity surrounded by the solidification shoe and the wheel groove, and then entering the extrusion shoe for extrusion and forming to obtain the first rod material; wherein, the casting temperature is 710°C, the cooling water temperature is 25°C, the extruded rod material diameter is 10mm, and the rod material temperature at the outlet is 500°C; the continuous casting and extrusion adopts the continuous casting and extrusion equipment conventionally used in the art, and the extrusion process adopts a three-outlet die, which can extrude three rod materials at the same time;

[0066] S5, rod quenching, using online cooling water to quench the first rod online, the water temperature is 25°C, and the extruded rod is rolled after online quenching and cooling;

[0067] S6, rod aging, the first rod is immediately subjected to aging treatment after quenching, the aging temperature is 180°C, the holding time is 15h, and the second rod obtained after aging contains dispersed β" (Mg5Si6) phase;

[0068] S7, rod drawing, using a sliding wire drawing machine to draw the second rod, the sliding wire drawing machine uses a nano-diamond composite coating die, the drawing speed is 11m / s, the final drawing dimensional accuracy is controlled within ±0.01mm, and a single wire diameter of 3.5mm is obtained. Aluminum alloy wire;

[0069] S8, single wire aging, aging treatment is performed on the aluminum alloy wire formed by drawing the rod, the temperature of the single wire aging is 150°C, the holding time is 7 hours, and a refined aluminum alloy wire is obtained after the single wire aging; wherein the remaining alloy elements in the refined aluminum alloy wire are further precipitated to form a second dispersed phase mainly composed of β" (Mg5Si6) and β' (Mg9Si5).

[0070] For the refined aluminum alloy wire in this embodiment, its single wire strength is measured by E45.504 tensile testing machine and is ≥316MPa; its conductivity is measured by PC36C DC resistance meter and is ≥57.6%IACS; its elongation is measured by electronic extensometer Y50 and is ≥5.8%.

[0071] Example 3

[0072] The present embodiment provides an aluminum alloy wire with high conductivity and high strength, which includes the following components by weight percentage: Mg 0.52%, Si 0.48%, Fe 0.15%, Y 0.22%, La 0.03%, B 0.006%, the balance being Al and unavoidable impurity elements, Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of impurity elements ≤0.02%.

[0073] The preparation method of the high-conductivity and high-strength aluminum alloy wire in this embodiment is as follows:

[0074] S1. Smelting: according to the element composition and weight percentage of the aluminum alloy wire, an aluminum ingot with a purity greater than 99.7%, an iron agent, a silicon agent, and an aluminum rare earth alloy are added into a smelting furnace, heated to melt, and then a magnesium ingot is added and melted, and a first melt is obtained after sufficient stirring;

[0075] S2, furnace refining, the first melt is transferred to a tilting holding furnace, a trace amount of aluminum-boron alloy is added for boronization treatment, the tilting holding furnace is turned on for full stirring, the melt temperature in the furnace is adjusted to 740°C for furnace refining for 15 minutes, and then the scum on the surface of the melt is thoroughly scraped off to obtain a second melt, the temperature of the second melt is adjusted to 725°C, and the melt is allowed to stand for 30 minutes;

[0076] S3, online refining, online degassing and online filtering of the second melt to obtain a third melt, wherein the online degassing adopts a rotary spray degassing box with high-purity nitrogen as the degassing medium, the speed of the graphite rotor is 450r / min, and the hydrogen content in the melt is made less than 0.12ml / 100g by online degassing; the online filtration adopts a two-stage foam ceramic filter box with a porosity of 30 / 50PPI to remove 5-10μm inclusion particles in the melt and reduce the adverse effect of inclusions on the elongation of the alloy single wire;

[0077] S4, continuous casting and extrusion, pouring the third melt into the rotating water-cooled groove wheel through the nozzle of the continuous casting and extrusion equipment, solidifying and forming in the cavity surrounded by the solidification shoe and the wheel groove, and then entering the extrusion shoe for extrusion and forming to obtain the first rod material; wherein, the casting temperature is 705°C, the cooling water temperature is 25°C, the extruded rod material diameter is 10mm, and the rod material temperature at the outlet is 498°C; the continuous casting and extrusion adopts the continuous casting and extrusion equipment conventionally used in the art, and the extrusion process adopts a three-outlet die, which can extrude three rod materials at the same time;

[0078] S5, rod quenching, using online cooling water to quench the first rod online, the water temperature is 25°C, and the extruded rod is rolled after online quenching and cooling;

[0079] S6, rod aging, the first rod is immediately subjected to aging treatment after quenching, the aging temperature is 195°C, the holding time is 14h, and the second rod obtained after aging contains dispersed β" (Mg5Si6) phase;

[0080] S7, rod drawing, using a sliding wire drawing machine to draw the second rod, the sliding wire drawing machine uses a nano-diamond composite coating die, the drawing speed is 12m / s, the final drawing dimensional accuracy is controlled within ±0.01mm, and a single wire diameter of 3.5mm is obtained. Aluminum alloy wire;

[0081] S8, single wire aging, aging treatment is performed on the aluminum alloy wire formed by drawing the rod, the temperature of the single wire aging is 155°C, the holding time is 7 hours, and a refined aluminum alloy wire is obtained after the single wire aging; wherein the remaining alloy elements in the refined aluminum alloy wire are further precipitated to form a second dispersed phase mainly composed of β" (Mg5Si6) and β' (Mg9Si5).

[0082] For the refined aluminum alloy wire in this embodiment, its single wire strength is measured by E45.504 tensile testing machine and is ≥335MPa; its conductivity is measured by PC36C DC resistance meter and is ≥57.1%IACS; its elongation is measured by electronic extensometer Y50 and is ≥5.2%.

[0083] Example 4

[0084] The present embodiment provides an aluminum alloy wire with high conductivity and high strength, which includes the following components by weight percentage: Mg 0.47%, Si 0.44%, Fe 0.13%, Y 0.3%, La 0.04%, B 0.02%, the balance being Al and unavoidable impurity elements, Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of impurity elements ≤0.02%.

[0085] The preparation method of the high-conductivity and high-strength aluminum alloy wire in this embodiment is as follows:

[0086] S1. Smelting: according to the element composition and weight percentage of the aluminum alloy wire, an aluminum ingot with a purity greater than 99.7%, an iron agent, a silicon agent, and an aluminum rare earth alloy are added into a smelting furnace, heated to melt, and then a magnesium ingot is added and melted, and a first melt is obtained after sufficient stirring;

[0087] S2, furnace refining, the first melt is transferred to a tilting holding furnace, a trace amount of aluminum-boron alloy is added for boronization treatment, the tilting holding furnace is turned on for sufficient stirring, the melt temperature in the furnace is adjusted to 730°C for furnace refining for 12 minutes, and then the scum on the surface of the melt is thoroughly scraped off to obtain a second melt, the temperature of the second melt is adjusted to 740°C, and the melt is allowed to stand for 25 minutes;

[0088] S3, online refining, online degassing and online filtering of the second melt to obtain a third melt, wherein the online degassing adopts a rotary spray degassing box with high-purity nitrogen as the degassing medium, the speed of the graphite rotor is 450r / min, and the hydrogen content in the melt is made less than 0.12ml / 100g by online degassing; the online filtration adopts a two-stage foam ceramic filter box with a porosity of 30 / 50PPI to remove 5-10μm inclusion particles in the melt and reduce the adverse effect of inclusions on the elongation of the alloy single wire;

[0089] S4, continuous casting and extrusion, pouring the third melt into the rotating water-cooled groove wheel through the nozzle of the continuous casting and extrusion equipment, solidifying and forming in the cavity surrounded by the solidification shoe and the wheel groove, and then entering the extrusion shoe for extrusion and forming to obtain the first rod material; wherein, the casting temperature is 710°C, the cooling water temperature is 20°C, the extruded rod material diameter is 10mm, and the rod material temperature at the outlet is 500°C; the continuous casting and extrusion adopts the continuous casting and extrusion equipment conventionally used in the art, and the extrusion process adopts a three-outlet die, which can extrude three rod materials at the same time;

[0090] S5, rod quenching, using online cooling water to quench the first rod online, the water temperature is 20°C, and the extruded rod is rolled after online quenching and cooling;

[0091] S6, rod aging, the first rod is immediately subjected to aging treatment after quenching, the aging temperature is 175°C, the holding time is 14h, and the second rod obtained after aging contains dispersed β" (Mg5Si6) phase;

[0092] S7, rod drawing, using a sliding wire drawing machine to draw the second rod, the sliding wire drawing machine uses a nano-diamond composite coating die, the drawing speed is 12m / s, the final drawing dimensional accuracy is controlled within ±0.01mm, and a single wire diameter of 3.5mm is obtained. Aluminum alloy wire;

[0093] S8, single wire aging, aging treatment is performed on the aluminum alloy wire formed by drawing the rod, the temperature of the single wire aging is 155°C, the holding time is 7 hours, and a refined aluminum alloy wire is obtained after the single wire aging; wherein the remaining alloy elements in the refined aluminum alloy wire are further precipitated to form a second dispersed phase mainly composed of β" (Mg5Si6) and β' (Mg9Si5).

[0094] For the refined aluminum alloy wire in this embodiment, its single wire strength is measured by E45.504 tensile testing machine and is ≥320MPa; its conductivity is measured by PC36C DC resistance meter and is ≥57.5%IACS; its elongation is measured by electronic extensometer Y50 and is ≥5.3%.

[0095] Comparative Example 1

[0096] This comparative example provides an aluminum alloy wire raw material with the same composition as that of Example 1, and the step of S6 rod aging is omitted in the preparation method. The remaining steps are also consistent with the preparation method in Example 1.

[0097] For the aluminum alloy wire in this comparative example, its single wire strength is measured by E45.504 tensile testing machine and is ≥334 MPa; its conductivity is measured by PC36C DC resistance meter and is ≥54.5% IACS; its elongation is measured by electronic extensometer Y50 and is ≥4.5%.

[0098] Comparative Example 2

[0099] The present embodiment provides an aluminum alloy wire, which includes the following components, by weight percentage: Mg 0.46%, Si 0.46%, Fe 0.14%, B 0.06%, the balance being Al and unavoidable impurity elements, Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, the total content of impurity elements ≤0.02%, and compared with Example 1, the two metal elements Y and La are not added.

[0100] The preparation method of the aluminum alloy wire in this comparative example is the same as that in Example 1.

[0101] For the aluminum alloy wire in this comparative example, its single wire strength is measured by E45.504 tensile testing machine and is ≥318 MPa; its conductivity is measured by PC36C DC resistance meter and is ≥56.4% IACS; its elongation is measured by electronic extensometer Y50 and is ≥5.8%.

[0102] Comparative Example 3

[0103] This comparative example provides an aluminum alloy wire, wherein the contents of each component are outside the scope of the claims, by weight percentage, specifically, comprising: Mg 0.36%, Si 0.35%, Fe 0.15%, Y 0.13%, La 0.02%, B 0.04%, the balance being Al and unavoidable impurity elements, Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of impurity elements ≤0.02%.

[0104] The preparation method of the aluminum alloy wire in this comparative example is the same as that in Example 1.

[0105] For the aluminum alloy wire in this comparative example, its single wire strength is measured by E45.504 tensile testing machine and is ≥296MPa; its conductivity is measured by PC36C DC resistance meter and is ≥57.5%IACS; its elongation is measured by electronic extensometer Y50 and is ≥6.6%.

[0106] The test results of Examples 1-3 indicate that the high-conductivity and high-strength aluminum alloy wire and the preparation method thereof provided by the present invention can achieve two excellent properties of high single-filament strength and high conductivity on the same aluminum alloy wire, thereby improving product quality and increasing its competitiveness in the market.

[0107] The experimental results of Example 1 and Comparative Example 1 show that if the aging step of the rod material is reduced, the first dispersed phase β" (Mg5Si6) and the second dispersed phase β' (Mg9Si5) will not be able to fully precipitate from the matrix, thereby affecting the strength and conductivity of the aluminum alloy wire, making it impossible to meet the performance of both at the same time.

[0108] The experimental results of Example 1 and Comparative Example 2 show that Y and La metal elements are essential components in the composition of the entire aluminum alloy wire. If the two are not doped, the number of crystal nucleation sites will be reduced and the structure cannot be refined, which will further affect the strength and conductivity of the aluminum alloy wire, making it impossible to meet the performance of both at the same time.

[0109] The experimental results of Example 1 and Comparative Example 3 show that the composition range of the high-conductivity and high-strength aluminum alloy wire provided by the present invention is optimal. If the proportion of each component is fine-tuned outside the composition range of the present invention, it will also affect the strength and conductivity of the aluminum alloy wire, making it impossible to meet the performance of both at the same time.

[0110] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A high-conductivity and high-strength aluminum alloy wire, characterized in that: The aluminum alloy wire comprises the following components by weight percentage: Mg 0.43-0.52%, Si 0.44-0.5%, Fe 0.12-0.15%, Y 0.18-0.3%, La 0.03-0.05%, B 0.005-0.02%, and the balance is Al and other impurity elements.

2. The high-conductivity and high-strength aluminum alloy wire according to claim 1, characterized in that: The weight percentages of the other impurity elements are: Ti≤0.005%, Mn≤0.005%, Cr≤0.005%, V≤0.005%, and the total content of the other impurity elements is ≤0.02%.

3. The high-conductivity and high-strength aluminum alloy wire according to claim 1, characterized in that: The aluminum alloy wire has a single-filament strength of ≥315 MPa, a conductivity of ≥57% IACS, and an elongation of ≥5%.

4. A method for preparing a high-conductivity and high-strength aluminum alloy wire as claimed in claims 1 to 3, characterized in that: The following steps are involved: S1, smelting, according to the element composition and weight percentage of the aluminum alloy wire, adding aluminum ingots, iron agent, silicon agent and aluminum rare earth alloy into a smelting furnace, heating and melting, then adding magnesium ingots, and fully stirring to obtain a first melt; S2, refining in a furnace, adding aluminum-boron alloy to the first melt for boronization treatment, stirring thoroughly and then standing to cool, to obtain a second melt; S3, online refining, performing online degassing and online filtering on the second melt to obtain a third melt; S4, continuous casting and extrusion, wherein the third melt is cooled and solidified by continuous casting and extrusion equipment, and then extruded to obtain a first rod material; S5, rod quenching, the first rod is subjected to online quenching cooling; S6, rod aging, the rod material after online quenching is immediately subjected to rod aging treatment at 160-200°C, and kept at this temperature for 10-18 hours to obtain a second rod material; S7, rod drawing, using a sliding wire drawing machine to draw the second rod after aging to obtain an aluminum alloy wire, wherein the diameter of the aluminum alloy wire is 2.5-4.0 mm; S8, single wire aging, the aluminum alloy wire is subjected to single wire aging treatment at 150-180° C. and kept warm for 7-10 hours to obtain a refined aluminum alloy wire.

5. The method for preparing a high-conductivity and high-strength aluminum alloy wire according to claim 4, characterized in that: In step S2, the stirring temperature of the furnace refining is 730-750°C, the stirring time of the furnace refining is 10-15 minutes, the standing temperature of the furnace refining is 720-730°C, and the standing time of the furnace refining is 25-40 minutes.

6. The method for preparing a high-conductivity and high-strength aluminum alloy wire according to claim 4, characterized in that: In step S3, the online degassing adopts a rotary spray degassing box, and the online filtration adopts a double-stage foam ceramic filter box.

7. The method for preparing a high-conductivity and high-strength aluminum alloy wire according to claim 6, characterized in that: The degassing medium of the rotary jet degassing box is high-purity nitrogen, and the rotation speed of the graphite rotor is 400-500r / min; the porosity of the double-stage foam ceramic filter box is 30-50PPI.

8. The method for preparing a high-conductivity and high-strength aluminum alloy wire according to claim 4, characterized in that: In step S4, the casting temperature of the continuous casting equipment is 690-710°C, the diameter of the first rod material is 9-10 mm, and the outlet temperature of the first rod material is 480-520°C.

9. The method for preparing a high-conductivity and high-strength aluminum alloy wire according to claim 4, characterized in that: In step S7, the drawing speed of the sliding wire drawing machine is 10-15 m / s, and the sliding wire drawing machine adopts a nano-diamond composite coating mold.

10. The method for preparing a high-conductivity and high-strength aluminum alloy wire according to claim 4, characterized in that: In steps S6 and S8, after rod aging, the first rod contains a first dispersed phase β" (Mg5Si6); after single wire aging, the first dispersed phase β" (Mg5Si6) and a second dispersed phase β' (Mg9Si5) are precipitated from the aluminum alloy wire.

Citation Information

Cited By

  • Aluminum alloy wire and method of making, aluminum alloy core aerial flame-retardant insulated cable

    CN122727583A