Al-Si sacrificial anode added with Mg, Ga and Zn for improving anode insufficiency and uneven corrosion
By adding Zn, Mg and Ga to the Al-10Si plating alloy, the sacrificial anode performance and corrosion uniformity are improved, and the problems of insufficient protection performance and uneven corrosion of the Al-10Si plating alloy in the prior art are solved, and the further development is achieved. Efficient steel component protection and alloy utilization.
Patent Information
- Application Number
- CN202410785718.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing hot-dip aluminum technology, the sacrificial anode protection performance of Al-10Si plating alloy is insufficient and the corrosion is uneven, which makes it difficult for corrosion products to fall off when adhered to the alloy surface, affecting production efficiency and alloy utilization.
Add appropriate amounts of Zn, Mg and Ga to the Al-10Si plating alloy to improve the physical and chemical properties of the alloy through solid solution and activation mechanisms, improve the sacrificial anode performance, and promote the uniform fall of corrosion products. The specific method includes melting the alloy in an oxygen-free well furnace, adding Al, Si, Fe, Mg, Zn and Ga arranged in weight percentage, stirring and pouring, to form a uniform plating alloy.
The sacrificial anode performance and corrosion resistance of Al-10Si plating alloy are significantly improved, corrosion uniformity and easy falloff of corrosion products are achieved, the strength and toughness of the alloy are improved, and production costs are reduced.
Smart Images

Figure CN118910475A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of steel anti-corrosion surface engineering, and in particular relates to an Al-Si sacrificial anode which is added with Mg, Ga and Zn to improve anode deficiency and uneven corrosion. Background Art
[0002] Hot-dip galvanizing is the main method for steel to deal with corrosion problems. It is widely used in many aspects of production and life, so the hot-dip galvanizing industry has developed on a large scale. However, limited zinc resources cannot meet the rapidly increasing demand for zinc consumption, and aluminum is the most promising new material for hot-dip plating of steel. Hot-dip aluminum has good protection for the steel substrate, but the aluminum coating is prone to generate dense oxides and passivation, which will result in insufficient sacrificial anode protection performance.
[0003] The iron and steel workpieces are wetted by the high temperature of the plating solution, and the iron elements in them will gradually penetrate into the plating solution. However, in order to pursue production efficiency, the industrialized continuous hot-dip aluminum production line often cannot replace the plating solution in time. As production proceeds, the iron content in the plating solution will gradually become saturated, that is, the mass percentage of Fe in the plating solution is close to 3.5. During the reaction process of continuous hot-dip aluminum plating, the Fe-Al-Si compound generated by the iron in the plating solution and the aluminum and silicon elements appears on the surface of the coating. The self-corrosion potential of the Fe-Al-Si compound is generally -310±30mVvs SCE, which is much higher than the Si phase electrode potential of -450±10mVvs SCE. After testing, when the Si content is added at 10wt.%, the τ6 phase formed with Al and Fe is beneficial to reduce the overall electrode potential of the alloy to a certain extent. The electrode potential of the α-Al matrix is -823mVvs SCE, which still does not meet the sacrificial anode driving potential requirements, directly affecting the application of continuous hot-dip aluminum alloy products. Therefore, the cathodic protection effect of Al-10Si coating alloy on steel components still needs to be further optimized. In the process of CN202211547246.1, the transformation of iron-containing intermetallic compounds is realized by variable temperature annealing, so that the grain of aluminum sacrificial anode coating is refined, and the anode performance and mechanical properties are improved. The main role of Zn is to enhance the reaction between the molten alloy and the steel, reduce the hot dip temperature, shorten the hot dip time, and shift the potential of the sacrificial anode coating negatively. Its variable temperature annealing is complicated, and the morphology of the alloy after corrosion is not considered. After adding Mg in CN202310569621.0, it mainly plays the role of preferential dissolution and activation of the second phase, but ignores the phenomenon that the activation element Mg may be deposited or segregated in large quantities at the grain boundary or in the grain of the alloy. This segregation will affect the mechanical properties of the alloy and the problem of uneven corrosion. Specifically, it may be manifested as a large amount of activation elements enriched at the grain boundary, which may lead to increased grain boundary brittleness and reduce the strength and toughness of the alloy.
[0004] When sacrificial anode is used, some corrosion products will adhere to the surface of the alloy and are difficult to fall off by themselves, resulting in obstruction of the sacrificial anode path and reduced efficiency. If manual treatment is used, production progress will be hindered and production costs will increase. After the corrosion resistance requirements of the sacrificial anode are met, the corrosion surface of the alloy is uniform during the corrosion process and the corrosion products are easy to fall off. If the corrosion products adhere to the substrate, the reaction will be hindered. On the other hand, they are easier to fall off to reduce the corrosion products and the corrosion inside the alloy, resulting in the failure of the protective substrate. The easy shedding of corrosion products is conducive to improving the utilization rate of the alloy. Summary of the invention
[0005] In order to solve the above problems, the present invention can effectively improve the sacrificial anode performance and edge protection performance of the Al-10Si coating alloy by adding appropriate amounts of Zn, Mg, Ga, and Fe, and the corrosion products are easy to fall off, achieving uniform corrosion, and is suitable for cathodic protection of steel components.
[0006] In order to study the morphology of the alloy after corrosion and whether the corrosion products are easy to fall off, the present invention adds Ga and Zn to Al-10Si. The existence form of Ga and Zn in the matrix is solid solution. The addition of Ga and Zn together can not only further improve the strength and hardness of the alloy as a whole, but also change the crystal structure of the alloy because Ga and Zn ions are solid dissolved in different vacancies of the matrix when added at the same time, making Cl - It is easier to penetrate, thus accelerating the corrosion rate. In addition, Mg is added to form a Mg2Si anode phase with Si. The three-element coupling of the two activation modes changes the physical and chemical properties of the alloy. The comprehensive use of these two activation mechanisms can improve the performance of the alloy more comprehensively, further improve the performance of the sacrificial anode and ensure the uniformity of the corrosion morphology. At the same time, the sacrificial anode protection performance and corrosion resistance of the coating alloy are improved, and the surface activity of the coating alloy under the iron saturation state is realized, and the sacrificial anode protection performance and corrosion resistance are greatly improved.
[0007] In order to achieve the above purpose, the technical method adopted by the present invention is:
[0008] The anode plating alloy provided by the invention comprises, by weight ratio of elements, 2% Zn, 1.5% Mg, 0.05-0.2% Ga, 10% Si, 0-3.5% Fe, and the rest Al and inevitable impurities.
[0009] As a preferred embodiment, the addition amount of Mg is 1.5%, the addition amount of Zn is 2.0%, and the addition amount of Ga is 0.1%. When the alloy content is Al-10Si-Fe-2Zn-1.5Mg-0.1Ga, the sacrificial anode performance requirements can be met, the structure is uniform, and the corrosion products are easy to fall off.
[0010] The present invention provides an Al-10Si-Fe-2Zn-1.5Mg-Ga anode coating alloy for continuous hot dip plating and a preparation method thereof, comprising the following steps:
[0011] (1) Melting of Al-10Si-Zn-Mg-Ga anode alloy for continuous hot dip plating:
[0012] In an oxygen-free pit furnace, under standard atmospheric pressure, dynamic argon and 4% hydrogen protection, the Al-Si master alloy is completely melted to remove the scum, then kept at 720°C for 10 minutes, and Al particles configured by weight percentage are added to prepare an Al-10Si alloy solution; then pure iron is added, kept at 800°C and stirred several times until the iron is completely melted; then pure magnesium, pure gallium, and pure zinc particles wrapped in aluminum foil are added in turn, stirred evenly, and kept warm for 20-30 minutes;
[0013] The silicon is added in the form of Al-12.24Si master alloy, and the purity of iron, magnesium, zinc and gallium are all greater than 99.9%.
[0014] Pure magnesium particles, pure zinc particles and pure gallium particles are wrapped with pure aluminum foil and pressed into the bottom of the alloy solution to reduce the consumption of zinc, magnesium and gallium.
[0015] (2) Preheat the cast iron mold at 400°C for 20 minutes before pouring.
[0016] (3) After the alloy solution is fully stirred, it is allowed to stand and keep warm for 30 minutes, and the surface scum is removed by a corundum tool, and the plated alloy solution is introduced into the mold and taken out after air cooling.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) In the art, the presence of Fe in aluminum-based anode materials is usually defined as an impurity harmful element. However, after adding 3.5wt.% of Fe to Al-10Si-2Zn-1.5Mg-0.1Ga, it was found that the corrosion potential of the Fe-containing alloy was more negative than that of the alloy without Fe, the sacrificial anode performance was better, and the alloy gradually changed from local uneven corrosion to comprehensive uniform corrosion. After adding Fe, Fe-Al-Si phase appeared in the alloy, and the corrosion rate of the alloy gradually increased with the extension of corrosion time, and there was almost no corrosion product film attached to the corrosion interface during the corrosion process. Therefore, the average corrosion rate of Al-10Si-3.5Fe-2Zn-1.5Mg-0.1Ga alloy was greater than that of Al-10Si-2Zn-1.5Mg-0.1Ga. After being corroded, the Fe-Al-Si compound was broken into small pieces, the corrosion products were not easy to adhere, and the integrity of the corrosion product film was reduced. This shows that the Fe element can accelerate the formation and peeling and dissolution of the corrosion product film on the alloy surface, which helps to improve the sacrificial anode performance of the plated alloy.
[0019] (2) Adding Zn can shift the self-corrosion potential of the coating alloy negatively, increase the self-corrosion current density, and improve the corrosion tendency of the coating alloy. The addition of Zn makes the dissolution more uniform. During the corrosion process, the aluminum matrix will be corroded first, generating flocculent corrosion products and controlling the corrosion rate. Secondly, a small amount of zinc dissolved in the Fe-Al-Si compound can promote pitting, thereby increasing the corrosion tendency. Mg can react with Si in the aluminum matrix to generate the Mg2Si anode phase, which is concentrated in the aluminum matrix. Because the electrode potential is relatively negative, it will be preferentially dissolved, accelerating the corrosion of the aluminum matrix. In the application of anodic protection of steel, another part of Mg in the coating alloy will also react with Al to generate the Chinese character-shaped π-Al9Si5Mg3Fe phase distributed around the Fe-Al-Si compound. Because the potential of this phase is relatively positive, it can be used as the anode phase and form galvanic corrosion with the Fe-Al-Si compound, increasing the corrosion tendency of the Fe-Al-Si compound. Further corrosion reactions occur inside the matrix, increasing the path to break through the external passivation film from the inside. The main activation mechanism of Ga is: "dissolution-redeposition". In the electrolyte, aluminum and Ga dissolved in the aluminum matrix are oxidized into ions and enter the solution. Ga cations obtain electrons from the aluminum matrix and deposit on the aluminum surface. The deposition of Ga cations dissolves the aluminum oxide film locally, thereby destroying the aluminum passivation film, activating the aluminum matrix, and forming pitting on the alloy surface. The pitting process can top the oxide film and expose the fresh matrix, thereby accelerating the self-corrosion of the aluminum alloy and improving the sacrificial anode capacity of the aluminum alloy.
[0020] (3) Compared with adding Zn or Ga alone, the co-addition of Zn and Ga not only further reduces the electronegativity, but also makes the microstructure more uniform and the corrosion more uniform. This is because the activation characteristics of Zn and Ga and the highly penetrating ions on the alloy surface cause it.
[0021] (4) The addition of Mg, Ga, and Zn will significantly reduce the charge transfer resistance of the coating and significantly destroy the passivation film, thereby increasing the active sites on the surface of the coating, breaking through the obstruction of the oxide film, and evenly dissolving the matrix, obtaining a relatively stable corrosion rate, improving the overall activity of the coating, and better realizing the cathodic protection effect; in addition, since Ga and Zn are solid dissolved in the matrix, and Mg promotes a more uniform overall structure of the alloy, fewer corrosion products are attached to the surface of the substrate, thereby reducing the problems of obstruction of the sacrificial anode path and reduced efficiency due to excessive corrosion products.
[0022] (5) The coupling of three elements in two activation modes changes the physical and chemical properties of the alloy. The comprehensive use of these two activation mechanisms can improve the performance of the alloy more comprehensively, further improve the performance of the sacrificial anode and ensure the uniformity of the corrosion morphology. The order of adding Mg, Ga, and Zn to the Al-10Si alloy is to add Mg first, then Ga, and finally Zn. The synergistic effect of Mg, Ga, and Zn in the Al-Si alloy is reflected in the promotion of the formation of eutectic phase and the formation of strengthening phases in the alloy. These strengthening phases can effectively inhibit intergranular corrosion and improve the strength of the alloy. When the alloy content is Al-10Si-2Zn-1.5Mg-0.1Ga, the sacrificial anode performance requirements for protecting steel components can be met, the organization is uniform, and the corrosion products are easy to fall off.
[0023] The method of the invention is simple to operate and low in cost, can well activate the Fe-Al-Si compound, and promotes uniform corrosion of the coating. The performance of the sacrificial anode is greatly improved, and the morphology of the alloy after corrosion is more uniform. It is of great significance to solve the practical problems of Fe-Al-Si and promote the use of continuous hot-dip aluminum plating. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The coating is the morphology after alloy corrosion;
[0025] Figure 2 Potentiodynamic polarization curves of Examples 1, 2, 3 and Comparative Example 1 in 3.5wt.% NaCl solution;
[0026] Figure 3 Open circuit potential diagrams of Examples 1, 2, 3 and Comparative Example 1 in 3.5wt.% NaCl solution;
[0027] Figure 4 The corrosion morphology of the cut edge after the cyclic corrosion test of the Al-10Si-3.5Fe-2.0Zn-1.5Mg-0.1Ga alloy in Example 2;
[0028] Figure 5 Corrosion morphology of Al-10Si-3.5Fe-2Zn-1.5Mg alloy in Comparative Example 1;
[0029] Figure 6 Corrosion morphology of Al-10Si-3.5Fe alloy in Comparative Example 4;
[0030] Figure 7 Corrosion morphology of Al-10Si-2.0Zn-1.5Mg-0.1Ga alloy in Comparative Example 6;
[0031] Figure 8Corrosion morphology of the cut edge after the cyclic corrosion test of the Al-10Si-2.0Zn-1.5Mg-0.1Ga alloy in Comparative Example 6. Specific implementation plan
[0032] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention, but do not constitute a limitation of the present invention.
[0033] Among them, 3.5wt.% is the maximum alloy "tolerance" of iron in aluminum alloy; silicon is added in the form of Al-12.24Si master alloy, and zinc, magnesium, gallium, iron, and aluminum are added in the form of single substances with a purity greater than 99.9%. The specific experimental steps are as follows.
[0034] Example 1
[0035] Preparation method of Al-10Si-3.5Fe-2Zn-1.5Mg-0.05Ga coating alloy, specific steps:
[0036] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 56.25g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. Then, 17.5g of pure iron is added, kept at 800℃ and stirred several times until the iron is completely melted. Then, pure magnesium, pure gallium particles and pure zinc wrapped in aluminum foil are added in turn, stirred evenly and kept warm for 10 minutes. 7.5g of pure magnesium particles, 0.25g of pure gallium particles and 10g of pure zinc particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of zinc, magnesium and gallium. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is allowed to stand and keep warm for thirty minutes, and the surface scum is removed by a corundum tool. The coating alloy solution is introduced into a mold, and taken out after air cooling to obtain the Al-10Si-3.5Fe-2Zn-1.5Mg-0.05Ga coating alloy.
[0037] Example 2
[0038] Preparation method of Al-10Si-3.5Fe-2Zn-1.5Mg-0.1Ga coating alloy, specific steps:
[0039] In an oxygen-free pit furnace under standard atmospheric pressure, dynamic argon and 4% hydrogen protection environment, 408.5g of Al-Si master alloy is completely melted to remove scum, then kept at 720°C for 10 minutes, 56g of Al particles configured by weight percentage are added to prepare Al-10Si alloy solution; then 17.5g of pure iron is added, kept at 800°C and stirred for multiple times until the iron is completely melted; then pure magnesium, pure gallium particles and pure zinc wrapped in aluminum foil are added in turn, stirred evenly and kept warm for 10 minutes; 7.5g of pure magnesium particles, 10g of pure zinc particles and 0.5g of pure gallium particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of zinc, magnesium and gallium. Before pouring, the cast iron mold is preheated at 400°C for 20 minutes; after the alloy solution is fully stirred, it is allowed to stand and keep warm for 30 minutes, the surface scum is removed by a corundum tool, the coating alloy solution is introduced into the mold, and taken out after air cooling, which is the Al-10Si-3.5Fe-2Zn-1.5Mg-0.1Ga coating alloy.
[0040] Figure 1 The morphology of the plated alloy after corrosion; (a) the surface morphology of the Al-10Si-3.5Fe-2.0Zn-1.5Mg-0.1Ga coating of Example 2 after immersion in 3.5wt.% NaCl solution for 24 hours; (b) an enlarged view of area I in Figure (a); (c) an enlarged view of area II in Figure (b); (e) the surface morphology of the α-Al region in the Al-10Si-3.5Fe-2.0Zn-1.5Mg-0.1Ga coating of Example 2 after immersion in 3.5wt.% NaCl solution for 72 hours. It can be seen that the surface morphology after immersion for different times has relatively few corrosion products on the surface. As the corrosion time increases, the α-Al region is corroded first, and the granular Mg2Si and Si phases are retained ( Figure 1 (c) This is because during the corrosion process, Mg2Si and Si phases are cathode phases, while α-Al phase is anode phase with a more negative corrosion potential. At the same time, the activation effect of Zn and Ga elements plays a promoting role.
[0041] Figure 1 (d) Surface morphology of Comparative Example 4Al-Si-3.5Fe after immersion in 3.5wt.% NaCl solution for 72h;
[0042] Figure 4 The corrosion morphology of the cut edge after the cyclic corrosion test of the Al-10Si-3.5Fe-2.0Zn-1.5Mg-0.1Ga alloy in Example 2;
[0043] Cyclic corrosion test conditions: Use a salt spray machine, place the prepared alloy at an angle of -30 degrees, use 5% NaCl solution for atomization spray, and the test temperature is 35°C. The volume of the salt spray box should be large enough, and do not spray the salt spray directly onto the test surface.
[0044] Figure 4 (a) Corrosion morphology of the cut edge at 0h after the cyclic corrosion test in Example 2; Figure 4 (b) Corrosion morphology of the cut edge 24 h after the cyclic corrosion test in Example 2; Figure 4 (c) Corrosion morphology of the cut edge after cyclic corrosion test in Example 2 for 72 h; Figure 4 (d) Corrosion morphology of the cut edge 120 h after the cyclic corrosion test in Example 2. Figure 8 (a) Corrosion morphology of the cut edge at 0h after the Al-10Si-2Zn-1.5Mg-0.1Ga cyclic corrosion test in comparative example 6; Figure 8 (b) Corrosion morphology of the cut edge 24 h after the cyclic corrosion test of Comparative Example 6; Figure 8 (c) Corrosion morphology of the cut edge after 72h of cyclic corrosion test in Comparative Example 6; Figure 8 (d) Corrosion morphology of the cut edge after 120 hours of cyclic corrosion test in Comparative Example 6. It can be concluded that the cut edge protection performance of the coating can be measured by the amount of corrosion products attached to the cut edge. Figure 4 It can be seen from (a)-(d) that as the corrosion time increases, the amount of corrosion products at the cut edge gradually increases. When the corrosion time reaches 120h, the cut edge is completely covered by corrosion products, and the Al-10Si-3.5Fe-2.0Zn-1.5Mg-0.1Ga corrosion products present a loose multi-crack structure. Compared with the Al-10Si-2.0Zn-1.5Mg-0.1Ga coating without Fe addition, the corrosion products are easy to fall off, reducing the problems of sacrificial anode pathway obstruction and reduced efficiency due to excessive corrosion products and difficulty in falling off.
[0045] Example 3
[0046] The preparation method of Al-10Si-3.5Fe-2Zn-1.5Mg-0.2Ga coating alloy specifically comprises the following steps:
[0047] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 55.5g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. Then, 17.5g of pure iron is added, kept at 800℃ and stirred several times until the iron is completely melted. Then, pure magnesium, pure gallium particles and pure zinc wrapped in aluminum foil are added in turn, stirred evenly and kept warm for 10 minutes. Pure 7.5g magnesium particles, 1.0g pure gallium particles and 10g pure zinc particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of zinc, magnesium and gallium. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is allowed to stand and keep warm for thirty minutes, and the surface scum is removed by a corundum tool. The coating alloy solution is introduced into a mold, and taken out after air cooling to obtain the Al-10Si-3.5Fe-2Zn-1.5Mg-0.2Ga coating alloy.
[0048] Comparative Example 1
[0049] The preparation method of Al-10Si-3.5Fe-2Zn-1.5Mg coating alloy specifically comprises the following steps:
[0050] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 56.5g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. Then, 17.5g of pure iron is added, kept at 800℃ and stirred several times until the iron is completely melted. Then, 7.5g of pure magnesium wrapped in aluminum foil is added, stirred evenly, and kept warm for 10 minutes. Then, 10g of pure zinc particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of zinc, magnesium and gallium. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is kept warm for 30 minutes. The surface scum is removed by corundum tools, and the coating alloy solution is introduced into the mold. After air cooling, it is taken out to obtain the Al-10Si-3.5Fe-2Zn-1.5Mg coating alloy.
[0051] Figure 5 The corrosion morphology of Al-10Si-3.5Fe-2Zn-1.5Mg alloy in Comparative Example 1; (a) 500μm morphology of Al-10Si-3.5Fe-2.0Zn-1.5Mg alloy after corrosion; (b) enlarged view of area I in (a); (c) enlarged view of area II in (a); (d) enlarged view of area III in (a); (e)-(f) are local element distribution diagrams of (b): (e) Si; (f) O. Due to the potential difference between the phases in the alloy, galvanic corrosion also exists in the alloy, such as Si and α-Al matrix ( Figure 5(c)), τ6 and α-Al matrix ( Figure 5 (d)). As pitting and galvanic corrosion progress, the oxide film and corrosion products on the alloy surface fall off, exposing new alloy. However, compared with Example 2 containing Ga, the corrosion uniformity of the alloy surface is not as good as that of Example 2 containing Ga.
[0052] The open circuit potential and polarization curve tests were carried out in a constant temperature water bath at room temperature using a three-electrode system in an electrochemical test system model PARSTAT-4000A. The saturated calomel electrode (SCE) was used as the reference electrode, the sample was used as the working electrode, the auxiliary electrode was a platinum electrode, and the surface area of the test anode was 1 cm 2 The sample was cut into 11mm×11mm horizontal lines, and then roughly polished to 10mm×10mm with acetone and 100-grit sandpaper. A hole was punched on one side of the sample to insert a wire of suitable size. The other side was cold-mounted with AB glue and a mounting mold. After the cold mounting was completed, it was further fine-ground with sandpaper (grade 400-1000-2000-), and then polished. After cleaning with alcohol and drying, the open circuit potential (OCP) and dynamic potential polarization curve (Tafel) were immediately tested.
[0053] First, the open circuit potential test was conducted at 25°C in a 3.5wt.% NaCl solution for 3600s. The dynamic potential polarization curve was finally scanned in the range of ±0.5V (vs. OCP) with a scanning speed of 1mV / s. The anode sample and the platinum electrode were in a 3.5wt.% NaCl solution for 2001s, and the polarization curve was finally fitted and analyzed using CView2 software. In addition, the samples after electrochemical corrosion were simply washed with deionized water and dried in a drying oven, and then the microstructure was further observed by SEM on the surface and interface.
[0054] Figure 2 Potentiodynamic polarization curves of Examples 1, 2, 3 and Comparative Example 1 in 3.5wt.% NaCl solution; With the increase of Ga content, the self-corrosion current density of Example 1 is 1.2×10 -6 ; Example 2 is 1.4×10 -6 ; Example 3 is 1.1×10 -6 ; Comparative Example 1 is 1.0×10 -6 , unit: A / cm 2 It can be seen that the self-corrosion potential first shifts negatively and then positively, and the self-corrosion current density first increases and then decreases, indicating that the corrosion tendency first increases and then decreases, that is, the corrosion rate first increases and then decreases, indicating that the sacrificial anode protection cathode performance of the Al-10Si-3.5Fe-2.0Zn-1.5Mg-0.1Ga coating is the best.
[0055] Figure 3The open circuit potential diagram of Examples 1, 2, 3 and Comparative Example 1 in 3.5wt.% NaCl solution shows that as the amount of Ga element added increases, the open circuit potential of the coating shifts first negatively and then positively after reaching a steady state. When the addition amount is 0.1wt.%, the open circuit potential in the equilibrium state is the most negative, about -1050mV.
[0056] Comparative Example 2
[0057] The preparation method of Al-10Si-3.5Fe-2Zn-0.1Ga coating alloy specifically comprises the following steps:
[0058] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 63.5g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. Then, 17.5g of pure iron is added, kept at 800℃ and stirred several times until the iron is completely melted. Then, 0.5g of pure gallium particles wrapped in aluminum foil are added, stirred evenly, and kept warm for 10 minutes. Then, 10g of pure zinc particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of zinc and gallium. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is kept warm for 30 minutes. The surface scum is removed by corundum tools, and the coating alloy solution is introduced into the mold. After air cooling, it is taken out, which is the Al-10Si-3.5Fe-2Zn-0.1Ga coating alloy.
[0059] Comparative Example 2 is Zn, Mg, and Ga, but only Zn and Ga are added in the absence of Mg. The electronegativity is sufficient, but the Mg2Si anode phase with a relatively negative electrode potential and the π-Al9Si5Mg3Fe distributed around the Fe-Al-Si compound are missing. This phase has a relatively positive potential and can be used as an anode phase. This phase can form galvanic corrosion with the Fe-Al-Si compound, which can increase the corrosion tendency of the Fe-Al-Si compound, thereby promoting further corrosion reactions inside the matrix. No Mg is added, which reduces the way to break through the external passivation film from the inside.
[0060] Comparative Example 3
[0061] The preparation method of Al-10Si-3.5Fe-1.5Mg-0.1Ga coating alloy specifically comprises the following steps:
[0062] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 66g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. Then, 17.5g of pure iron is added, kept at 800℃ and stirred several times until the iron is completely melted. Then, 7.5g of pure magnesium wrapped in aluminum foil is added, stirred evenly, and kept warm for 10 minutes. Then, 0.5g of pure gallium particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of magnesium and gallium. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is kept warm for 30 minutes. The surface scum is removed by corundum tools, and the coating alloy solution is introduced into the mold. After air cooling, it is taken out, which is the Al-10Si-3.5Fe-1.5Mg-0.1Ga coating alloy.
[0063] In comparative example 3, only Ga and Mg are added, and the lack of Zn leads to poor electronegativity reduction effect, small electronegativity reduction, and decreased overall activation characteristics of the alloy.
[0064] Comparative Example 4
[0065] The preparation method of Al-10Si-3.5Fe coating alloy specifically comprises the following steps:
[0066] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 74g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. Then, 17.5g of pure iron is added, and the mixture is kept at 800℃ and stirred several times until the iron is completely melted. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is kept still for 30 minutes, and the surface scum is removed by corundum tools. The coating alloy solution is introduced into the mold, and taken out after air cooling, which is the Al-10Si-3.5Fe coating alloy.
[0067] Comparative Example 4 is that none of the three elements Zn, Mg and Ga are added. Figure 6 From the corrosion morphology of the Al-10Si-3.5Fe alloy in Example 4, it was found that the corrosion was localized non-uniform corrosion.
[0068] Comparative Example 5
[0069] Comparative Example 5 is an Al-10Si-3.5Fe-2Zn-1.5Mg-0.1Mn alloy. Compared with Example 2, Ga is replaced with an equal amount of Mn. The results show that Mn is mainly distributed in Fe-Al-Si and does not form a second phase. However, it is not as active as Ga and is not as effective as Ga in reducing the electrode potential.
[0070] Comparative Example 6
[0071] The preparation method of Al-10Si-2Zn-1.5Mg-0.1Ga coating alloy specifically comprises the following steps:
[0072] In an oxygen-free pit furnace, 408.5g of Al-Si master alloy is completely melted and scum is removed in an environment protected by dynamic argon and 4% hydrogen at standard atmospheric pressure. Then, 73.5g of Al particles are added according to weight percentage to prepare Al-10Si alloy solution. After heating to 800℃, pure magnesium, pure gallium particles and pure zinc wrapped in aluminum foil are added in sequence, stirred evenly, and kept warm for 10 minutes. 7.5g of pure magnesium particles, 0.5g of pure gallium particles and 10g of pure zinc particles are wrapped in pure aluminum foil and pressed into the alloy solution to reduce the consumption of zinc, magnesium and gallium. The cast iron mold is preheated at 400℃ for 20 minutes before pouring. After the alloy solution is fully stirred, it is kept warm for 30 minutes. The surface scum is removed by corundum tools, and the coating alloy solution is introduced into the mold. After air cooling, it is taken out to obtain the Al-10Si-2Zn-1.5Mg-0.1Ga coating alloy.
[0073]
[0074] Figure 7 The corrosion morphology of the Al-10Si-2.0Zn-1.5Mg-0.1Ga coating alloy in Comparative Example 6 (a) is an electron microscope image at 100 μm; (b) is an electron microscope image at 50 μm; (c) is an electron microscope image at 10 μm; Figure 7 For comparative example 6, an alloy containing three elements coupled but not containing Fe is added. Figure 1 By adding the alloy containing Fe in the three-element coupling of Example 2, the two were compared and found that: under the same corrosion environment, the Al-10Si-3.5Fe-2Zn-1.5Mg-0.1Ga alloy of Example 2 has fewer corrosion products, which are easier to fall off and dissolve more evenly. This shows that the multi-element coupling effect promotes the formation of more activation points in the oxide film on the surface of the alloy, breaks through the obstruction of the oxide film on the surface, causes the matrix to dissolve evenly, and obtains a stable corrosion rate.
[0075] The morphology of the Al-10Si-3.5Fe-2Zn-1.5Mg-0.1Ga plated alloy after corrosion is the most uniform and dense, and the electrode potential is also the most negative of all the embodiments, reaching -1.0V, which is within the optimal standard range of the sacrificial anode reference in the application of the alloy to protect steel. At the same time, the corrosion products are dense and easy to fall off, reducing the reduction in efficiency due to excessive enrichment and the greatly weakened metal protection ability due to excessive intermetallic corrosion. This embodiment is the optimal metal composition ratio that meets the protection conditions.
[0076] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, or modification made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An Al-Si sacrificial anode with addition of Mg, Ga and Zn for improving anode deficiency and uneven corrosion, characterized in that: The following components are present in percentage by weight Composition: Silicon 10%, zinc 2%, magnesium 1.5%, gallium 0.05-0.2%, iron 0-3.5%, the rest is Al and inevitable impurities.
2. The method for preparing an Al-Si sacrificial anode with addition of Mg, Ga and Zn for improving anode deficiency and uneven corrosion according to claim 1, characterized in that: The preparation steps are as follows: (1) Alloy melting After the Al-Si master alloy is completely melted and the scum is removed, Al particles are added to prepare an Al-10Si alloy solution after keeping the temperature for a period of time; pure iron is added, kept at 800°C and stirred several times until the iron is completely melted; then pure magnesium, pure gallium particles and pure zinc wrapped in aluminum foil are pressed into the bottom in turn, and after they are melted, they are stirred evenly and left to stand and keep the temperature; (2) Mold preheating After the alloy in step (1) is completely melted, it is poured into a preheated cast iron mold, air-cooled, refined and cast into a billet; (3) Remove surface impurities by slag removal, remove gas and slag by desiccant, pour the coating alloy solution into the mold, air cool, refine and cast into billet.
3. The method for preparing an Al-Si sacrificial anode for improving anode deficiency and uneven corrosion by adding Mg, Ga and Zn according to claim 2, characterized in that: The melting temperature of the Al-Si master alloy in step (1) is 720° C.; the insulation condition is 720° C. for 10 min; the melting environment in step (1) is carried out under the protection of standard atmospheric pressure, dynamic argon and 4% hydrogen.
4. The method for preparing an Al-Si sacrificial anode with addition of Mg, Ga and Zn for improving anode deficiency and uneven corrosion as claimed in claim 2, characterized in that: In step (1), the purity of pure iron, magnesium particles, zinc particles and gallium particles is greater than 99.9%.
5. The method for preparing an Al-Si sacrificial anode with addition of Mg, Ga and Zn for improving anode deficiency and uneven corrosion as claimed in claim 2, characterized in that: The Al-Si master alloy in step (1) is an Al-Si alloy containing 12.24wt.% Si, which is configured according to mass percentage and then smelted in an oxygen-free pit furnace.
6. Application of the Al-Si sacrificial anode with added Mg, Ga and Zn as claimed in claim 1 in cathodic protection of steel workpieces.
7. The use according to claim 6, characterized in that: The alloy composition of the coating after application is 10% silicon, 2% zinc, 1.5% magnesium, 0.05-0.2% gallium, 0-3.5% iron, and the rest is Al and inevitable impurities; the harmful effect of iron element in the steel workpiece in the sacrificial anode is avoided.
Citation Information
Cited By
Praseodymium modified secondary aluminum alkaline air battery anode material and preparation method thereof