High-conductivity heat-resistant aluminum alloy conductor and preparation method thereof
By optimizing the composition and process flow of aluminum alloy, the problem of insufficient conductivity and heat resistance of aluminum alloy conductors is solved, and the preparation of high-conductivity and heat-resistant aluminum alloy conductors is realized, simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202410999172.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
The existing aluminum alloy wires have limitations in conductivity and heat resistance, and the preparation process is complex, making it difficult to meet industrial standards under high loads and special environments.
By optimizing the alloy composition, adding elements such as Zr, Fe, Si, Mg, B and RE, the aluminum alloy liquid is deeply purified, and a resistance furnace melting, degassing, filtration and heat treatment processes are used to prepare high-conductivity and heat-resistant aluminum alloy wires.
The heat resistance and strength of aluminum alloy wires are significantly improved, the preparation process is simplified, making them suitable for industrial production, and the material cost is reduced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy wire preparation, in particular to a high-conductivity heat-resistant aluminum alloy wire and a preparation method thereof. Background Art
[0002] With the rapid development of modern power systems, the performance requirements for transmission wires are getting higher and higher. Especially under high load and special environments, such as high temperature and strong corrosion, traditional wire materials can no longer meet the increasingly stringent industrial standards and usage requirements. As a medium for power transmission, the conductivity and heat resistance of wires are directly related to the operating efficiency, safety and stability of the power grid.
[0003] At present, the common wire materials on the market mainly include pure aluminum wire, copper wire and some aluminum alloy wire. Pure aluminum wire has good conductivity, but its heat resistance and mechanical properties are relatively poor, especially when running under high load, it is easy to cause safety hazards due to thermal expansion. Although copper wire has excellent conductivity and good heat resistance, its high cost, heavy weight, and difficult installation and maintenance limit its application in specific occasions. Aluminum alloy wire combines the advantages of aluminum and copper, with good conductivity and high strength, but due to the addition of alloy elements, its conductivity is lower than that of pure aluminum, and the heat resistance of different aluminum alloys varies greatly.
[0004] The aluminum alloy wires in the prior art still have certain limitations in conductivity and heat resistance, which are mainly manifested in the following aspects: insufficient conductivity, limited heat resistance, complex preparation process, and insufficient corrosion resistance. Summary of the invention
[0005] In view of the above deficiencies in the prior art, the purpose of the present invention is to provide a high-conductivity heat-resistant aluminum alloy wire, by optimizing the alloy composition, improving the heat resistance and strength of the aluminum alloy wire, by deeply purifying the aluminum alloy liquid, improving the conductivity of the aluminum alloy wire, and obtaining a high-conductivity heat-resistant aluminum alloy wire.
[0006] Another object of the present invention is to provide a method for preparing a high-conductivity heat-resistant aluminum alloy wire, which has a simple preparation method, mild process conditions, and is conducive to industrial production.
[0007] The present invention is achieved by adopting the following technical solutions:
[0008] The high-conductivity heat-resistant aluminum alloy wire is composed of the following elements in percentage by weight: Zr: 0.03-0.09%; Fe: 0.05-0.2%; Si: 0.05-0.1%; Mg: 0.60-0.90%; B: 0.03-0.09%; RE: 0.05-0.1%, and the rest is aluminum.
[0009] The RE is composed of the following elements: Ce: 25-35%; La: 68-75%.
[0010] The method for preparing the high-conductivity heat-resistant aluminum alloy wire comprises the following steps:
[0011] (1) According to the composition and mass percentage of the aluminum alloy conductor, aluminum silicon alloy, aluminum iron alloy, magnesium boron alloy, aluminum ingot with a purity of ≥99.7% and mixed rare earth RE mainly composed of La and Ce are selected as raw materials for batching;
[0012] (2) placing the ingredients obtained in step (1) in a resistance furnace for melting, wherein the temperature of the aluminum liquid after melting is 720° C.-750° C.;
[0013] (3) then adding aluminum-zirconium master alloy and aluminum-cerium master alloy to the aluminum liquid, and after the master alloy is melted, stirring it fully, refining and degassing it with high-purity argon gas, removing slag and letting it stand;
[0014] (4) The aluminum alloy liquid in the furnace flows through a double-rotor degassing box arranged on a flow trough for online degassing outside the furnace;
[0015] (5) passing the aluminum alloy liquid through a double filter plate filter box arranged on a flow trough for off-furnace online filtering treatment;
[0016] (6) Then entering the continuous casting and rolling production line at 750°C-780°C to cast aluminum alloy bars;
[0017] (7) hot rolling the aluminum alloy cast strip on a hot rolling mill to produce heat-resistant aluminum alloy rods through an aluminum continuous casting and rolling production line;
[0018] (8) The aluminum alloy rod is heat treated, and the heat-treated aluminum alloy rod is drawn and stranded to produce high-strength, high-conductivity, and heat-resistant aluminum alloy wires.
[0019] The cerium Ce has almost no solid solution in the aluminum Al, and the micron-sized eutectic Al is formed during the subsequent hot rolling and wire drawing process. 11 The Ce3 phase is broken into particles.
[0020] The weight percentage of zirconium in the aluminum-zirconium master alloy is 6.88%.
[0021] The weight percentage of cerium in the aluminum-cerium master alloy is 25%.
[0022] The aluminum alloy cast strip is hot rolled on a hot rolling mill, wherein the rolling temperature is 540°C-545°C.
[0023] The aluminum alloy rod is heat treated at a temperature of 350° C.-450° C. and for a time of 3-8 hours.
[0024] Aluminum itself has high electrical conductivity and is an excellent conductor material. By precisely controlling the content of other elements, the conductivity of the conductor can be maintained or improved. The addition of Zr (zirconium) and Mg (magnesium) can improve the heat resistance of the alloy, so that the conductor still maintains good mechanical and electrical properties in high temperature environments. Mg is usually used to improve the strength and toughness of aluminum alloys, so that the conductor has better tensile strength and fatigue resistance. The addition of Ce (cerium) and RE (other rare earth elements) can significantly improve the physical and chemical properties of the alloy. Rare earth elements can refine the grains, improve the strength and toughness of the conductor, and may also improve the corrosion resistance and oxidation resistance of the conductor. B (boron) is usually used as a grain refiner in aluminum alloys, which helps to improve the processing properties of the alloy and makes the conductor easier to form during processing. The appropriate addition of Fe (iron) and Si (silicon) may improve the corrosion resistance of the conductor, especially in an environment containing Fe. The addition of iron helps to form a dense oxide film and improve the protective performance of the conductor. By precisely controlling the content of each element, the microstructure of the alloy can be optimized, segregation and defects can be reduced, and the uniformity and reliability of the conductor can be improved. The addition of zirconium and rare earth elements helps to improve the stability of the alloy at high temperatures and reduce softening and creep phenomena at high temperatures. Through reasonable alloy design, the conductor can maintain good performance under different environmental conditions, including extreme temperatures and corrosive environments. By optimizing the alloy composition, the material cost can be reduced without sacrificing performance, and the economic benefits of the conductor can be improved.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention promotes the precipitation and stabilization of Al3Zr particles in the aluminum matrix by adding mixed rare earth RE mainly composed of La and Ce, and then refines and modifies the coarse Fe-rich phase so that the Fe-rich phase is dispersed in the aluminum matrix and grain boundaries in the form of fine particles, thereby significantly improving the heat resistance and strength of the aluminum alloy wire; 5%-12% of cerium Ce is used. Since Ce has almost no solid solution in Al, it will form an Al11Ce3 eutectic phase with Al during the solidification process. In the subsequent rolling and drawing process, the micron-sized eutectic Al 11 The Ce3 phase is broken into particles, which can pin the grain boundaries, improve strength and inhibit recrystallization softening.
[0027] (2) The present invention improves the heat resistance and strength of the aluminum alloy wire by optimizing the alloy composition, and improves the conductivity of the aluminum alloy wire by deeply purifying the aluminum alloy liquid, thereby obtaining a high-conductivity heat-resistant aluminum alloy wire.
[0028] (3) The preparation method of the present invention is simple, the process conditions are relatively mild, and it is conducive to industrial production. DETAILED DESCRIPTION
[0029] In order to make the purpose and technical solution of the present invention more clear, the present invention is further described in detail below.
[0030] Example 1
[0031] The high-conductivity heat-resistant aluminum alloy wire is composed of the following elements in percentage by weight: Zr: 0.03%; Si: 0.05%; Mg: 0.60%; B: 0.03%; RE: 0.05%, and the rest is aluminum.
[0032] A method for preparing a high-conductivity heat-resistant aluminum alloy wire comprises the following steps:
[0033] (1) According to the composition and mass percentage of the aluminum alloy conductor, aluminum silicon alloy, magnesium boron alloy, aluminum iron alloy, aluminum ingot with a purity of ≥99.7% and mixed rare earth RE mainly composed of La and Ce are selected as raw materials for batching;
[0034] (2) placing the ingredients obtained in step (1) in a resistance furnace for melting, wherein the temperature of the aluminum liquid after melting is 750° C.;
[0035] (3) then adding aluminum-zirconium master alloy and aluminum-cerium master alloy to the aluminum liquid, and after the master alloy is melted, stirring it fully, refining and degassing it with high-purity argon gas, removing slag and letting it stand;
[0036] (4) The aluminum alloy liquid in the furnace flows through a double-rotor degassing box arranged on a flow trough for online degassing treatment outside the furnace;
[0037] (5) passing the aluminum alloy liquid through a double filter plate filter box arranged on a flow trough for off-furnace online filtering treatment;
[0038] (6) Then entering the continuous casting and rolling production line at 780°C to cast aluminum alloy bars;
[0039] (7) hot rolling the aluminum alloy cast strip on a hot rolling mill to produce heat-resistant aluminum alloy rods through an aluminum continuous casting and rolling production line;
[0040] (8) The aluminum alloy rod is heat treated, and the heat-treated aluminum alloy rod is drawn and stranded to produce high-strength, high-conductivity, and heat-resistant aluminum alloy wires.
[0041] The test results are shown in Table 1.
[0042] Example 2
[0043] The high-conductivity heat-resistant aluminum alloy wire is composed of the following elements in percentage by weight: Zr: 0.09%; Fe: 0.2%; Si: 0.1%; Mg: 0.90%; B: 0.09%; RE: 0.1%, and the rest is aluminum.
[0044] A method for preparing a high-conductivity heat-resistant aluminum alloy wire comprises the following steps:
[0045] (1) According to the composition and mass percentage of the aluminum alloy conductor, aluminum silicon alloy, aluminum iron alloy, magnesium boron alloy, aluminum ingot with a purity of ≥99.7% and mixed rare earth RE mainly composed of La and Ce are selected as raw materials for batching;
[0046] (2) placing the ingredients obtained in step (1) in a resistance furnace for melting, wherein the temperature of the aluminum liquid after melting is 720° C.;
[0047] (3) then adding aluminum-zirconium master alloy and aluminum-cerium master alloy to the aluminum liquid, and after the master alloy is melted, stirring it fully, refining and degassing it with high-purity argon gas, removing slag and letting it stand;
[0048] (4) The aluminum alloy liquid in the furnace flows through a double-rotor degassing box arranged on a flow trough for online degassing outside the furnace;
[0049] (5) passing the aluminum alloy liquid through a double filter plate filter box arranged on a flow trough for off-furnace online filtering treatment;
[0050] (6) Then entering the continuous casting and rolling production line at 750°C to cast aluminum alloy bars;
[0051] (7) hot rolling the aluminum alloy cast strip on a hot rolling mill to produce heat-resistant aluminum alloy rods through an aluminum continuous casting and rolling production line;
[0052] (8) The aluminum alloy rod is heat treated, and the heat-treated aluminum alloy rod is drawn and stranded to produce high-strength, high-conductivity, and heat-resistant aluminum alloy wires.
[0053] The test results are shown in Table 1.
[0054] Example 3
[0055] The high-conductivity heat-resistant aluminum alloy wire is composed of the following elements in percentage by weight: Zr: 0.03%; Fe: 0.05%; Si: 0.05%; Mg: 0.60%; B: 0.03%; RE: 0.05%, and the rest is aluminum.
[0056] A method for preparing a high-conductivity heat-resistant aluminum alloy wire comprises the following steps:
[0057] (1) According to the composition and mass percentage of the aluminum alloy conductor, aluminum silicon alloy, aluminum iron alloy, magnesium boron alloy, aluminum ingot with a purity of ≥99.7% and mixed rare earth RE mainly composed of La and Ce are selected as raw materials for batching;
[0058] (2) placing the ingredients obtained in step (1) in a resistance furnace for melting, wherein the temperature of the aluminum liquid after melting is 720° C.;
[0059] (3) then adding aluminum-zirconium master alloy and aluminum-cerium master alloy to the aluminum liquid, and after the master alloy is melted, stirring it fully, refining and degassing it with high-purity argon gas, removing slag and letting it stand;
[0060] (4) The aluminum alloy liquid in the furnace flows through a double-rotor degassing box arranged on a flow trough for online degassing treatment outside the furnace;
[0061] (5) passing the aluminum alloy liquid through a double filter plate filter box arranged on a flow trough for off-furnace online filtering treatment;
[0062] (6) Then entering the continuous casting and rolling production line at 750°C to cast aluminum alloy bars;
[0063] (7) hot rolling the aluminum alloy cast strip on a hot rolling mill to produce heat-resistant aluminum alloy rods through an aluminum continuous casting and rolling production line;
[0064] (8) The aluminum alloy rod is heat treated, and the heat-treated aluminum alloy rod is drawn and stranded to produce high-strength, high-conductivity, and heat-resistant aluminum alloy wires.
[0065] The test results are shown in Table 1.
[0066] Table 1 Test results of Examples 1-3
[0067]
[0068]
Claims
1. A high-conductivity heat-resistant aluminum alloy wire, It is characterized in that It is composed of the following elements in percentage by weight: Zr: 0.03-0.09%; Fe: 0.05-0.2%; Si: 0.05-0.1%; Mg: 0.60-0.90%; B: 0.03-0.09%; RE: 0.05-0.1%, and the rest is aluminum.
2. The high-conductivity heat-resistant aluminum alloy wire according to claim 1, It is characterized in that The RE is composed of the following elements: Ce: 25-35%; La: 68-75%.
3. A method for preparing the high-conductivity heat-resistant aluminum alloy wire according to claim 1 or 2, It is characterized in that The steps include: (1) According to the composition and mass percentage of the aluminum alloy conductor, aluminum silicon alloy, magnesium boron alloy, aluminum iron alloy, aluminum ingot with a purity of ≥99.7% and mixed rare earth RE mainly composed of La and Ce are selected as raw materials for batching; (2) placing the ingredients obtained in step (1) in a resistance furnace for melting, wherein the temperature of the aluminum liquid after melting is 720-750° C.; (3) then adding aluminum-zirconium master alloy and aluminum-cerium master alloy to the aluminum liquid, and after the master alloy is melted, stirring it fully, refining and degassing it with high-purity argon gas, removing slag and letting it stand; (4) The aluminum alloy liquid in the furnace flows through a double-rotor degassing box arranged on a flow trough for online degassing treatment outside the furnace; (5) passing the aluminum alloy liquid through a double filter plate filter box arranged on a flow trough for off-furnace online filtering treatment; (6) Then entering the continuous casting and rolling production line at 750-780°C to cast aluminum alloy bars; (7) hot rolling the aluminum alloy cast strip on a hot rolling mill to produce heat-resistant aluminum alloy rods through an aluminum continuous casting and rolling production line; (8) The aluminum alloy rod is heat treated, and the heat-treated aluminum alloy rod is drawn and stranded to produce high-strength, high-conductivity, and heat-resistant aluminum alloy wires.
4. The method for preparing the high-conductivity heat-resistant aluminum alloy wire according to claim 3, It is characterized in that The Ce is almost not dissolved in aluminum Al, and the micron-sized eutectic Al 11 Ce 3 Phase broken into particles.
5. The method for preparing the high-conductivity heat-resistant aluminum alloy wire according to claim 3, It is characterized in that The weight percentage of zirconium in the aluminum-zirconium master alloy is 6.88%.
6. The method for preparing the high-conductivity heat-resistant aluminum alloy wire according to claim 3, It is characterized in that The weight percentage of cerium in the aluminum-cerium master alloy is 25%.
7. The method for preparing the high-conductivity heat-resistant aluminum alloy wire according to claim 3, It is characterized in that The aluminum alloy cast strip is hot rolled on a hot rolling mill, wherein the rolling temperature is 540-545°C.
8. The method for preparing the high-conductivity heat-resistant aluminum alloy wire according to claim 3, It is characterized in that The aluminum alloy rod is heat treated at a temperature of 350-450° C. and for a time of 3-8 hours.