800MPa-grade magnetic pole steel for pumped storage hydroelectric generating set and production method of 800MPa-grade magnetic pole steel
Through specific chemical composition and process flow, the problem of difficulty in producing 800MPa grade magnetic pole steel in the existing technology is solved, and the production of magnetic pole steel with high strength, high elongation and good magnetic inductance is achieved, reducing costs and meeting the pumped storage energy The demand for hydroelectric units.
Patent Information
- Application Number
- CN202410978174.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The prior art is difficult to produce 800MPa grade magnetic pole steel with a thickness of ≤2.0 mm, yield strength ≥800MPa, tensile strength ≥850MPa, elongation A ≥12%, and magnetic inductance B50 ≥1.6T, and the cost is relatively high.
Specific chemical composition combinations and process flows are adopted, including casting blank heating, 7-pass hot rolling, laminar cooling, winding, annealing and straightening, and the control element content is such as C: 0.25-0.30%, Si: 0.10-0.20 %, Mn: 1.1 to 1.5%, Cr: 0.2 to 0.3%, Ti: 0.1 to 0.2%, B: 0.0025 to 0.0030%, P: ≤0.015%, S: ≤0.010%, and through deep desulfurization pretreatment, it can reduce Use of precious metals such as Nb and Mo.
The production of 800MPa grade magnetic pole steel with thickness ≤2.0mm, yield strength ≥800MPa, tensile strength ≥850MPa, elongation A≥12%, magnetic inductance B50≥1.6T was achieved, reducing alloy cost and meeting high rotation speed The demand for pumped storage water-electric unit.
Smart Images

Figure BDA0004955205230000061 
Figure BDA0004955205230000062 
Figure BDA0004955205230000071
Abstract
Description
Technical Field
[0001] The present invention relates to a steel for motor and a production method thereof, and specifically to a 800MPa grade magnetic pole steel for pumped storage hydroelectric generator sets and a production method thereof. Background Art
[0002] Pumped-storage power stations are the green, low-carbon, clean and flexible power sources in the current power system with the most mature technology, the best economy and the best conditions for large-scale development. They work well with wind power, solar power generation, nuclear power, thermal power, etc.
[0003] Magnetic pole steel is used for the rotor magnetic pole part of the pumped storage generator structure. It is the main component of the hydro-turbine generator to generate the magnetic field. It is a rotating component and requires good electromagnetic and mechanical properties. The thickness is generally ≤2.0mm. As the rated speed of the unit increases, the strength requirements of the required magnetic pole steel plate also increase. Therefore, for the pumped storage hydro-turbine generator unit with a rated speed of 600r / min, the demand for extremely thin magnetic pole steel with a yield strength of ≥800MPa and a thickness of ≤2.0mm is proposed.
[0004] After searching:
[0005] The document with Chinese patent application number CN201210165348.7 discloses "A method for manufacturing high magnetic induction and low cost 250MPa cold-rolled magnetic pole steel", whose process includes: heating the slab to 1200-1260℃ and keeping it warm; hot rolling: the final rolling temperature is 850-900℃, the coiling temperature is 550-630℃, and the cooling method is jet water cooling; cooling to 60-80℃ for pickling, and the cooling method is air cooling; cold rolling: the cold rolling reduction rate is 50-75%; continuous annealing: the soaking section temperature is 720-780℃, and the soaking time is 60-200s; flattening is performed with a flattening elongation of 0.8-1.4%, and a 250MPa cold-rolled magnetic pole steel is produced. However, the yield strength of the produced magnetic pole steel is only 250MPa.
[0006] The document with Chinese patent application number CN200910049782.7 discloses "A method for manufacturing 500MPa grade cold-rolled magnetic pole steel", and the weight percentages of the main chemical components of the slab are: C: 0.07-0.10%, Si: 0.18-0.31%, Mn: 1.00-1.50%, P: ≤0.02%, S: ≤0.007%, O≤0.004%, N≤0.004%, Nb: 0.046-0.060%, Ti: ≤0.003%, V: 0.050-0.070%, and the remainder is Fe and unavoidable impurities. The process is as follows: (1) heating the slab to 1200-1260°C, rolling the slab into a thin steel plate, the final rolling temperature is 830-890°C, cooling to 550-600°C by laminar cooling for coiling; (2) air cooling and pickling; (3) cold rolling; (4) continuous annealing: the temperature of the annealing furnace soaking section is controlled at 740-760°C, the speed of the annealing process section is controlled at 120-125 m / min, and the soaking section time is controlled at 230-239s; (5) flattening. However, the yield strength of the product can only reach 570MPa.
[0007] The document with Chinese patent application number ZL202110575161.3 discloses a "Yoke Steel with Excellent Fatigue Resistance and Tensile Strength ≥850MPa", whose chemical composition and weight percentage are: C: 0.03-0.07%, Si: ≤0.15%, Mn: 0.5-1.0%, P: ≤0.015%, S: ≤0.002%, Nb: 0.075-0.095%, V: 0.015-0.025%, Mo: 0.20-0.30%, Als: 0.02-0.10%, N: ≤0.010%, and the rest is Fe and unavoidable impurities. Although its yield strength is close to ≥800MPa, it also contains precious metals such as Mo, Nb, and V, resulting in high alloy cost. Summary of the invention
[0008] The present invention aims to overcome the shortcomings of the prior art and provide a magnetic field having a thickness of ≤2.0mm, a yield strength of ≥800MPa, a tensile strength of ≥850MPa, an elongation of A≥12%, and a magnetic induction performance of B 50 800MPa grade magnetic pole steel for pumped storage hydroelectric units ≥1.6T and production method thereof.
[0009] Measures to achieve the above objectives:
[0010] The invention discloses an 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set, wherein the components and weight percentage contents thereof are as follows: C: 0.25-0.30%, Si: 0.10-0.20%, Mn: 1.1-1.5%, Cr: 0.2-0.3%, Ti: 0.1-0.2%, B: 0.0025-0.0030%, P: ≤0.015%, S: ≤0.010%, Als: 0.02-0.10%, and the rest are Fe and unavoidable inclusions.
[0011] Preferably, the weight percentage of Cr is 0.23-0.27%.
[0012] Preferably, the weight percentage of Ti is 0.1-0.15%.
[0013] A method for producing 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set, comprising the following steps:
[0014] 1) After conventional smelting, the billet is cast into a billet, during which the billet thickness is controlled to be 60-85 mm;
[0015] 2) Heat the ingot, control the soaking temperature at 1150-1200°C, and control the soaking time to be no less than 30 minutes;
[0016] 3) Use 7 passes of hot rolling to the product thickness: control the starting rolling temperature to be no less than 1050°C, and the final rolling temperature to be between 850 and 900°C;
[0017] 4) laminar cooling at a cooling rate of 50-70°C / s to the coiling temperature;
[0018] 5) Coil the steel sheet and control the coiling temperature at 400-500°C.
[0019] 6) Annealing is performed, and the annealing heating temperature is controlled to be 600-640° C. and the holding time is 3-6 hours;
[0020] 7) Perform straightening.
[0021] Preferably, the soaking temperature of the casting is between 1157°C and 1192°C.
[0022] Preferably, the starting rolling temperature is not less than 1058°C, and the final rolling temperature is between 868°C and 892°C.
[0023] Functions and mechanisms of each element and main process in the present invention
[0024] The carbon (C) content of the present invention is 0.25% to 0.30%, and carbon is the most economical strengthening element. However, if the carbon content is between 0.07% and 0.15%, the molten steel will undergo peritectic reaction during the casting process, increasing the risk of continuous casting leakage, and too high a carbon content will reduce the magnetic induction performance. Therefore, limiting the carbon content to 0.25% to 0.30% can not only improve the strength of the steel, but also ensure the magnetic induction performance of the steel, while greatly reducing the addition of alloy elements and reducing costs.
[0025] The manganese (Mn) content of the present invention is 1.1% to 1.5%. Manganese can reduce the phase transition temperature of austenite to ferrite, expand the hot working temperature range, and is conducive to refining the ferrite grain size and improving the yield strength of steel.
[0026] The chromium (Cr) content of the present invention is 0.2% to 0.3%: chromium is a carbide-forming element, has a strong affinity with carbon, and can hinder the diffusion of carbon atoms. Cr is beneficial to refine ferrite grains and improve the strength of steel plates, but too high a content is detrimental to magnetic properties. In the present invention, the chromium content is controlled at 0.2% to 0.3%, preferably: the weight percentage content of Cr is 0.23% to 0.27%.
[0027] The titanium (Ti) content of the present invention is 0.1% to 0.2%. Ti is a strong carbide and nitride forming element. The carbon and nitride particles formed can prevent the austenite grains from growing during the reheating of the steel and the rough rolling in the high-temperature austenite zone, play a role in refining the grains and improving the toughness of the steel. The fine dispersed TiC precipitated in the coiling stage can have a significant precipitation strengthening effect, thereby effectively improving the strength of the steel plate. The present invention selects a Ti content of 0.1% to 0.2%, preferably: the weight percentage content of Ti is 0.10% to 0.15%.
[0028] The silicon (Si) content of the present invention is 0.10% to 0.20%. Si has a solid solution strengthening effect, which can improve the strength of steel and is beneficial to magnetic properties. When the silicon content exceeds a certain range, it will be detrimental to the surface quality. Therefore, the present invention controls the Si content to 0.10% to 0.20%.
[0029] The phosphorus (P) content of the present invention is ≤0.015%, and the sulfur (S) content is ≤0.010%. Phosphorus in steel has adverse effects such as easily causing segregation and reducing magnetic induction performance. Sulfur is easily combined with manganese to form MnS inclusions, which affect the magnetic induction performance and plasticity of steel. Therefore, the present invention should minimize the adverse effects of phosphorus and sulfur elements on steel properties, and control the phosphorus and sulfur contents by means of deep desulfurization pretreatment of molten iron, thereby reducing their adverse effects.
[0030] The boron (B) content of the present invention is 0.0025% to 0.0030%. The main function of B is to act as a surface active element, adsorb on the austenite grain boundary, delay the transformation of austenite to ferrite, thereby refining the final structure and achieving a strengthening effect. In addition, B is extremely cheap and has a significant effect on cost control. However, if the B content is too high, a low melting point eutectic will be formed, which is concentrated on the grain boundary, thereby causing hot brittleness. Therefore, the boron content of the present invention is in the range of 0.0025% to 0.0030%.
[0031] The reason why the present invention controls the soaking temperature of the casting billet at 1150-1200°C is to ensure complete solid solution and sufficient austenitization of the alloy elements, while improving the uniformity of the slab temperature, reducing deformation resistance and rolling load, and facilitating the rolling of thin-gauge yoke steel.
[0032] The reason why the final rolling temperature is controlled at 850-900°C, the cooling rate is 50-70°C / s, and the coiling temperature is 400-500°C is to obtain a bainite structure by a high cooling rate, give full play to the structure strengthening and fine grain strengthening effects, and at the same time, through the annealing temperature of 600-640°C, TiC particles are fully precipitated, give full play to the precipitation strengthening effect, and improve the strength of the steel plate.
[0033] The present invention does not contain precious alloy elements such as Nb and Mo, and has a yield strength of ≥800MPa, an elongation A of ≥12%, and a magnetic induction performance B 50 ≥1.60T can fully meet and is applicable to the demand for 800MPa grade magnetic pole steel for pumped storage turbine generator rotor with a rated speed of 600r / min. The product thickness is no more than 2mm, and the cost can be reduced by 600 to 900 yuan / ton of steel compared with the existing technology. DETAILED DESCRIPTION
[0034] The present invention is described in detail below:
[0035] Table 1 is a list of component values of various embodiments and comparative examples of the present invention;
[0036] Table 2 is a table of process parameter values and performance tests for various embodiments and comparative examples of the present invention.
[0037] Each embodiment of the present invention is produced according to the following steps:
[0038] 1) After conventional smelting, the billet is cast into a billet, during which the billet thickness is controlled to be 60-85 mm;
[0039] 2) Heat the ingot, control the soaking temperature at 1150-1200°C, and control the soaking time to be no less than 30 minutes;
[0040] 3) Use 7 passes of hot rolling to the product thickness: control the starting rolling temperature to be no less than 1050°C, and the final rolling temperature to be between 850 and 900°C;
[0041] 4) laminar cooling at a cooling rate of 50-70°C / s to the coiling temperature;
[0042] 5) Coil the steel sheet and control the coiling temperature at 400-500°C.
[0043] 6) Perform annealing, control the annealing heating temperature to 600-640°C, and the insulation time to 3-6h; 7) Perform straightening.
[0044] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0045]
[0046] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0047]
[0048]
[0049] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0050]
[0051] It can be seen from Table 3 that the yield strength of each embodiment 1 to 8 is ≥800MPa, the elongation A is ≥12%, and the magnetic induction performance B is 50 ≥1.60T meets the market demand, and the hot-rolled plate thickness is rolled to no more than 2mm.
[0052] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. An 800MPa grade magnetic pole steel for a pumped storage hydroelectric unit, wherein the components and weight percentage contents are: C: 0.25-0.30%, Si: 0.10-0.20%, Mn: 1.1-1.5%, Cr: 0.2-0.3%, Ti: 0.1-0.2%, B: 0.0025-0.0030%, P: ≤0.015%, S: ≤0.010%, Als: 0.02-0.10%, and the rest is Fe and unavoidable inclusions.
2. The 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set according to claim 1, characterized in that: The weight percentage of Cr is 0.23-0.27%.
3. The 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set according to claim 1, characterized in that: The weight percentage of Ti is 0.1-0.15%.
4. A method for producing a 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 1, comprising the following steps: 1) After conventional smelting, the billet is cast into a billet, during which the billet thickness is controlled to be 60-85 mm; 2) Heat the ingot, control the soaking temperature at 1150-1200°C, and control the soaking time to be no less than 30 minutes; 3) Use 7 passes of hot rolling to the product thickness: control the starting rolling temperature to be no less than 1050°C, and the final rolling temperature to be between 850 and 900°C; 4) laminar cooling at a cooling rate of 50-70°C / s to the coiling temperature; 5) Coil the steel sheet and control the coiling temperature at 400-500°C. 6) Annealing is performed, and the annealing heating temperature is controlled to be 600-640° C. and the holding time is 3-6 hours; 7) Perform straightening.
5. The method for producing 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 4, characterized in that: The uniform heating temperature of the ingot is between 1157 and 1192°C.
6. The method for producing 800MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 4, characterized in that: The starting rolling temperature is not lower than 1058°C, and the final rolling temperature is between 868 and 892°C.
Citation Information
Patent Citations
Hot rolled steel in C-Mn-Ti series with high intensity magnetic induction performance
CN101003879A
Hot-rolled pole sheet steel and manufacturing method thereof
CN105624556A
High strength silicon steel sheet, and its production method
JP2005113184A
Steel pipe having superior electromagnetic property and manufacturing method therefor
JP2005281853A
Cited By
800 mpa-grade magnetic pole steel for pumped storage hydroelectric generating unit and production method
WO2026016356A1