Track shoe for large bulldozer and preparation method of track shoe

By optimizing the chemical composition and process flow, the problem of bainitic structure in the track plates of large bulldozers under low-temperature conditions was solved, and a ferrite + pearlite structure was achieved, which improved the hardenability and surface quality of the track plates and extended their service life.

CN118910506AActive Publication Date: 2024-11-08SHANDONG IRON & STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411289548.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-08
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

Existing technologies for manufacturing large bulldozer track plates at low temperatures suffer from poor machinability and surface defects due to bainitic microstructure, as well as insufficient hardenability, which affects the service life and processing quality of the track plates.

Method used

By optimizing the chemical composition and process flow, controlling the content of elements such as C, Si, Mn, Cr, B, Ti, Al, N, H, O, and As, and employing processes such as slow cooling pits, end electromagnetic stirring, and high-pressure water descaling, the track plates are ensured to have a ferrite + pearlite microstructure in a low-temperature environment, thereby improving hardenability and surface quality.

Benefits of technology

It achieves good processing performance of track plates in low-temperature environments, improves hardenability and wear resistance, reduces surface defects, and extends the service life of track plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910506A_ABST
    Figure CN118910506A_ABST
Patent Text Reader

Abstract

The track shoe comprises the following chemical components in percentage by weight: 0.25 to 0.31 percent of C, 0.36 to 0.80 percent of Si, 1.15 to 1.30 percent of Mn, less than or equal to 0.015 percent of P, less than or equal to 0.010 percent of S, 0.70 to 0.90 percent of Cr, 0.0015 to 0.0030 percent of B, 0.025 to 0.055 percent of Ti, 0.02 to 0.05 percent of Al, 0.003 to 0.006 percent of N, less than or equal to 0.0002 percent of H, less than or equal to 0.0025 percent of O, less than or equal to 0.0080 percent of As and the balance of iron and trace impurities, and the C range of the same cross section is less than or equal to 0.03 percent, the Mn range of the same cross section is less than or equal to 0.04 percent, and the Cr range of the same cross section is less than or equal to 0.05 percent. The hardenability value of the steel plate is 40HRClt; j25 is less than or equal to 45 HRC, 36 HRClt; and J30 < = 42 HRC. According to the method, the metallographic structures obtained after hot rolling and natural cooling of the track shoe at the low environment temperature (below 0 DEG C) in winter are ferrite and pearlite, bainite structures with poor toughness do not exist, good shearing and punching performance is achieved, meanwhile, the hardenability, the abrasion resistance and the fatigue resistance of the track shoe are further improved, and the service life of the track shoe is prolonged. And surface defects are effectively controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material metallurgy, and in particular, relates to a track shoe for a large bulldozer and a preparation method thereof. Background Art

[0002] Track shoes are divided into single-tooth, two-tooth, and three-tooth types to meet the needs of different machine models and working conditions. Bulldozers often use single-tooth track shoes. Track shoes have a variety of manufacturing processes such as casting, stamping, machining, and rolling. Compared with other methods, rolling has the characteristics of high efficiency, low cost, and excellent comprehensive performance, and has become the mainstream process for track shoe manufacturing. However, for the super-large single-tooth track plates used in large bulldozers, not only is rolling difficult, but the hardenability requirements for the material are also higher than those of ordinary track plates. To solve this problem, CN202210783391.3 discloses a high-hardenability steel section for super-large engineering machinery tracks and a production method thereof. The track steel section is composed of the following chemical components by weight percentage: C 0.23-0.30%, Si 0.15-0.35%, Mn 1.05-1.35%, P≤0.025%, S≤0.015%, Cr 0.60-0.90%, B0.0010-0.0030%, Ti 0.015-0.055%, Al 0.01-0.06%, and the rest is iron and unavoidable impurities. By increasing the Cr content from 0.3% to 0.60-0.90%, the hardenability and wear resistance are improved. Since the Cr element can significantly change the cooling transformation behavior of steel materials, as the Cr content increases, the continuous cooling transformation curve of steel shifts to the right, and the critical cooling rate of bainite transformation decreases, resulting in changes in the microstructure of the track plate under natural cooling conditions after rolling in winter with low ambient temperatures (below 0°C), resulting in bainite with poor plasticity, cracking during shearing and punching, resulting in insufficient environmental adaptability of the patented technology. On the other hand, in order to solve the problem that brittle phases such as Widmanstätten structure and bainite are prone to appear in the metallographic structure after the Cr content is increased, this patent adopts a lower final rolling temperature (not more than 930°C). Not only does it need to wait for the temperature before finishing rolling, which affects the rolling rhythm and reduces production efficiency, but also for high hardenability steel, at such a low final rolling temperature, the head of the rolled piece with a faster temperature drop is very likely to form martensite under the action of cooling water, making the hardness significantly higher than the hardness of the roll, resulting in pits on the roll surface when the head of the rolled piece bites into it, and forming rolling marks on the rolled piece during subsequent rolling. Surface defects. Summary of the invention

[0003] To solve the deficiencies of the existing technologies, the present invention provides a crawler shoe for a large bulldozer and a preparation method thereof, which can achieve that all the metallographic structures obtained by natural cooling after hot rolling of the crawler shoe in winter with a relatively low ambient temperature (below 0 °C) are ferrite + pearlite, without the bainite structure with poor toughness, and have good shearing and punching properties. At the same time, the hardenability, wear resistance, and fatigue resistance of the crawler shoe are further improved, and surface defects are effectively controlled.

[0004] To achieve the above object, the present invention adopts the following solutions:

[0005] A crawler shoe for a large bulldozer, the weight percentages of its chemical components are: C: 0.25 - 0.31%, Si: 0.36 - 0.80%, Mn: 1.15 - 1.30%, P ≤ 0.015%, S ≤ 0.010%, Cr: 0.70 - 0.90%, B: 0.0015 - 0.0030%, Ti: 0.025 - 0.055%, Al: 0.02 - 0.05%, N: 0.003 - 0.006%, H ≤ 0.0002%, O ≤ 0.0025%, As ≤ 0.0080%, and the rest is iron and trace impurities. The C range in the same cross-section ≤ 0.03%, the Mn range ≤ 0.04%, and the Cr range ≤ 0.05%.

[0006] For the crawler shoe involved in the present invention, its hardenability value is 40HRC < J25 ≤ 45HRC, 36HRC < J30 ≤ 42HRC, enabling the crawler shoe to have a thicker hardened layer depth and better wear resistance.

[0007] The crawler shoe for a large bulldozer provided by the present invention has a plate width of 300 - 400 mm, an equivalent thickness of the tooth root of 40 - 60 mm, a tooth height of 85 - 120 mm, and a web thickness of 20 - 40 mm.

[0008] As a preferred embodiment, the weight percentages of the chemical components of the crawler shoe for a large bulldozer are: C: 0.26 - 0.29%, Si: 0.40 - 0.70%, Mn: 1.15 - 1.25%, P ≤ 0.013%, S ≤ 0.008%, Cr: 0.75 - 0.85%, B: 0.0015 - 0.0025%, Ti: 0.03 - 0.05%, Al: 0.02 - 0.04%, N: 0.003 - 0.005%, H ≤ 0.0002%, O ≤ 0.0020%, As ≤ 0.0080%, and the rest is iron and trace impurities. The C range in the same cross-section ≤ 0.02%, the Mn range ≤ 0.03%, and the Cr range ≤ 0.04%.

[0009] C: C is the most economical element used to improve the strength of steel, but as the C content increases, the toughness of the steel will deteriorate. C is also the main element to increase the surface hardness after quenching, which can significantly improve the wear resistance of the surface and increase the service life of the material. After comprehensive consideration, it is determined that the C content is controlled within the range of 0.25% to 0.31%.

[0010] Si: Si is a deoxidizer that must be added during the steelmaking process. A small amount of Si will remain in the molten steel after deoxidation. After cooling, it can be dissolved in ferrite to increase strength and wear resistance. Experimental studies have shown that when the Si content in steel is low (less than 1%), as the Si content increases, the continuous cooling transformation curve of the steel will shift to the left, and the critical cooling rate of bainite transformation will increase, which is opposite to the effect of Cr on the continuous cooling transformation curve. Therefore, the present invention increases the Si content to 0.36-0.80%, thereby offsetting the bainite problem caused by the increase in Cr elements in low temperature environments. At the same time, the increase in Si content can also improve the hardenability of the steel, thereby increasing the J30 value and extending the service life of the track shoe.

[0011] Mn: has a solid solution strengthening effect and can improve strength. Mn can also combine with S to generate MnS, which improves the plasticity of steel at high temperatures and prevents hot cracks during the continuous casting process. However, Mn is an element that easily segregates. Adding too much will cause serious segregation in the core of the ingot, resulting in performance deterioration. Therefore, the present invention controls the Mn content within the range of 1.15-1.30%.

[0012] P: an inevitable impurity element brought by the ore. For the present invention, P is a harmful element that will reduce the toughness of the material and cause cold brittleness. Its content should be reduced as much as possible during the smelting process. However, removing the P element will increase the cost. Under the premise of not affecting the toughness, P≤0.015% is sufficient.

[0013] S: An inevitable impurity element brought by the ore. For the present invention, S is a harmful element that will reduce the high temperature toughness of the material and cause hot brittleness. S is also one of the main sources of inclusions in steel. Its content should be reduced as much as possible during the smelting process, or more Mn elements should be added to eliminate its hot brittleness. Under the premise of not affecting the use, S≤0.010% is sufficient.

[0014] Cr: a common alloying element in steel, Cr can increase the strength of steel, improve hardenability, and enhance wear resistance. It can also significantly change the cooling transformation behavior of steel materials. As the Cr content increases, the continuous cooling transformation curve of steel shifts to the right, making it easy to form bainite, resulting in processing cracking. The present invention increases the Si content on the basis of existing technology to offset the effect of Cr on bainite transformation. Therefore, the present invention controls the Cr content within the range of 0.70-0.90%.

[0015] B: It is an unavoidable residual element in metallurgical auxiliary materials. It has a great influence on the toughness of steel. B element tends to be concentrated at the grain boundary, reducing the low-temperature impact toughness of steel. However, B is also an element that effectively improves the hardenability. Adding a small amount can significantly improve the hardenability of steel. Considering comprehensively, the content of B element is controlled within the range of 0.0015-0.0030%.

[0016] Ti: Ti is more active than B and is easier to combine with N to fix nitrogen, thereby increasing the content of acid-soluble B. Under the condition of the same B content, adding Ti element can further improve the hardenability, but too high Ti content will deteriorate the toughness and cause the track shoe to crack. Controlling the Ti element content within the range of 0.025-0.055% can effectively improve the hardenability without reducing the toughness.

[0017] Al: Al is a common element for deoxidation of molten steel. It can combine with O in steel to form Al2O3, which is removed from the molten steel by floating, thus preventing B from losing its ability to improve hardenability due to oxidation. In addition, Al has an adverse effect on the castability of molten steel. Excessive addition can easily lead to nozzle blockage. Taking all factors into consideration, the Al content is controlled within the range of 0.02-0.05%.

[0018] N: N can promote the precipitation of microalloying elements such as Nb, V, and Ti to improve strength, and can also combine with Al to form AlN on the austenite grain boundary, inhibiting grain growth and improving toughness, but too much N will lead to strain aging and cause brittle fracture of steel after processing. Through experimental research and comparison, controlling the N content in the range of 0.003-0.006% can achieve the best match between track shoe strength and toughness.

[0019] H: H is a harmful element in steel, which causes defects such as cracks and white spots inside the steel, seriously reducing the toughness of the steel. Therefore, H must be controlled at an extremely low level. Controlling the H element content within the range of ≤0.0002% can meet the use needs of the track shoe.

[0020] O: O is a harmful element in steel and often exists in the form of inclusions, which destroys the continuity of the steel matrix and causes toughness and fatigue failure. However, in order to control the C content in steel, oxygen must be blown during steelmaking, resulting in a certain amount of O in the molten steel, which is removed by refining in the later stage. In order to meet the toughness and fatigue requirements and meet economical production, the present invention controls the O content within the range of ≤0.0025%.

[0021] As: An unavoidable harmful element that significantly reduces the toughness of steel. As is a common associated element in iron ore and enters molten steel from molten iron during the smelting process. To meet the use requirements of track shoes, As content should be controlled at ≤0.0080%.

[0022] The range is a parameter that characterizes the degree of segregation of the steel (or ingot) composition. A smaller range indicates that the steel (or ingot) composition is more uniform, and there is no situation where the content of elements such as C, Mn, Cr in local areas is higher than that in the matrix. In order to control the generation of abnormal tissues (bainite, martensite, etc.) during the cooling process and taking into account the guarantee capability of the preparation method of the present invention, it is specified that the C range is ≤0.03%, the Mn range is ≤0.04%, and the Cr range is ≤0.05%.

[0023] The present invention also provides a method for preparing the above-mentioned crawler shoe for a large bulldozer, comprising the following steps:

[0024] Step S1: using low-As molten iron and scrap steel for converter smelting and LF+vacuum refining, the As content in the molten iron is ≤80ppm, and the molten iron accounts for no less than 80% of the raw materials for converter steelmaking;

[0025] Step S2: using a continuous casting machine to cast a steel billet, the continuous casting machine is provided with an end electromagnetic stirring, the current is 450A-600A, and the straightening roll of the continuous casting machine is provided with a pressing function, and the pressing amount is 5-15mm;

[0026] Step S3: Slowly cooling the steel billet in a slow cooling pit;

[0027] Step S4: The steel billet is heated, rolled and cooled to form a track shoe.

[0028] Furthermore, in the above-mentioned preparation method, in the step S3, the slow cooling pit is first baked, and after the pit wall temperature reaches 750°C, the high-temperature steel billet off the continuous casting line is placed in the slow cooling pit for slow cooling to reduce the temperature gradient between the pit wall and the steel billet; after the slow cooling time is greater than 24h to 48h, the billet is taken out of the slow cooling pit to uniform the composition of the steel billet, reduce the segregation in the core, and prevent the appearance of abnormal structures such as bainite and martensite in the core due to the higher content of C, Mn and Cr elements than the surrounding areas.

[0029] Furthermore, in the above-mentioned preparation method, in the step S4, the steel billet is rough-rolled in 9 to 13 passes in the rolling process, among which there are 1 to 2 scaling passes to loosen and peel off the iron oxide scale on the surface of the rolled piece, and a steel turning operation (≥90°) is added after the scaling pass to remove the loosened and peeled iron oxide scale from the rolled piece, thereby compensating for the deficiency that the iron oxide scale is tightly adhered and difficult to remove by high-pressure water descaling, resulting in pits formed in the finished product due to the pressing of the iron oxide scale, thereby improving the surface quality of the track shoe.

[0030] Furthermore, in the above-mentioned preparation method, in the step S4, the final rolling temperature is 940-1000° C. Without low-temperature rolling, a full ferrite+pearlite structure can be obtained, thereby achieving efficient production and high surface quality of the track shoe.

[0031] The invention aims at the problem that the increase of Cr element leads to the formation of bainite structure in the track plate under low temperature environment, which deteriorates the processing performance. By increasing the Si element content, the adverse effect of Cr is compensated, and the prepared track plate structure can be all ferrite + pearlite; the increase of Si content further improves the hardenability of steel, increases the depth of hardened layer, and increases the wear resistance of track plate. The use of low As molten iron smelting can significantly reduce the risk of track plate fracture. The continuous casting adopts end electromagnetic stirring and controls the current at 450A to 600A, which can reduce the element segregation in the core, increase the proportion of equiaxed crystals, and improve toughness. By slowly cooling the billet, the element segregation in the core of the billet can be further eliminated, the extreme difference of C, Mn, and Cr elements can be reduced, and the generation of abnormal structures such as bainite can be prevented, so as to better ensure that the track plate structure after hot rolling is all ferrite + pearlite. The continuous casting billet is pressed down by 5-15mm in height by a straightening machine, and the positive temperature gradient of the billet can be used to achieve high penetration deformation, eliminate casting defects in the central area of ​​the billet, and improve the fatigue life of the track plate. The process of descaling and steel turning during the rolling process can further reduce the residual iron oxide scale after high-pressure water descaling and improve the surface quality of the track shoe. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the cross-sectional shape of a single-tooth track shoe;

[0033] 1——single-tooth track shoe;

[0034] 11 – tooth tip;

[0035] 12 – tooth root;

[0036] D——equivalent thickness of tooth root;

[0037] Figure 2 The track shoe structure prepared by the existing technology (more bainite exists);

[0038] Figure 3 The track shoe structure (without bainite) is prepared by the technology of the present invention;

[0039] Figure 4 The metallographic structure (without bainite) of the center part of the track shoe is prepared by the technology of the present invention. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0041] A track shoe for a large bulldozer (see attached Figure 1 ) and its preparation method, its chemical composition is compared with the existing large-size track shoe composition as shown in Table 1:

[0042] Table 1 Comparison of chemical composition of existing technology and track shoe of the present invention (wt%)

[0043]

[0044] Compared with the prior art, the chemical composition of the present invention further requires that the C extreme difference of the same cross section of the steel is ≤0.03%, the Mn extreme difference is ≤0.04%, and the Cr extreme difference is ≤0.05%.

[0045] Examples 1-3

[0046] The method for preparing the track shoe for a large bulldozer having the chemical composition of Examples 1-3 as shown in Table 2 comprises the following steps:

[0047] Step S1: using low-As molten iron and scrap steel for converter smelting and LF+vacuum refining, the As content in the molten iron is ≤80ppm, and the mass proportion of the molten iron in the raw materials for converter steelmaking is not less than 80%;

[0048] Step S2: using a continuous casting machine to cast a steel billet, the continuous casting machine is provided with an end electromagnetic stirring, the current is 450A-600A, and the straightening roll of the continuous casting machine is provided with a pressing function, and the pressing amount is 5-15mm;

[0049] Step S3: Slowly cooling the steel billet in a slow cooling pit;

[0050] Step S4: The steel billet is heated, rolled and cooled to form a track shoe. Figure 1 shown.

[0051] In step S3, the slow cooling pit is first baked, and after the pit wall temperature reaches 750°C, the high-temperature steel billet off the continuous casting line is placed in the slow cooling pit for slow cooling to reduce the temperature gradient between the pit wall and the steel billet; after the slow cooling time is greater than 24h to 48h, the billet is taken out of the slow cooling pit to make the composition of the steel billet uniform, reduce the segregation in the core, and prevent the appearance of abnormal structures such as bainite and martensite in the core due to the higher content of C, Mn and Cr elements than the surrounding areas.

[0052] In step S4, the steel billet is rough rolled in 9 to 13 passes in the rolling process, wherein 1 to 2 scale breaking passes are performed to loosen and peel off the iron oxide scale on the surface of the rolled piece, and a steel turning operation (≥90°) is added after the scale breaking passes to remove the loosened and peeled iron oxide scale from the rolled piece, thereby compensating for the defect that the iron oxide scale is tightly adhered and difficult to remove by high-pressure water descaling, resulting in pits formed in the finished product due to the pressing of the iron oxide scale, thereby improving the surface quality of the track shoe.

[0053] In step S4, the final rolling temperature is 940-1000° C. Without low-temperature rolling, a full ferrite+pearlite structure can be obtained, thereby achieving efficient production and high surface quality of the track shoe.

[0054] Table 2 Chemical composition of the track shoes for large bulldozers prepared in Examples 1-3 (wt%)

[0055]

[0056] Table 3 Composition difference of track shoes for large bulldozers prepared in Examples 1-3 (wt%)

[0057] chemical composition C Mn Cr Example 1 0.02 0.03 0.04 Example 2 0.02 0.02 0.03 Example 3 0.01 0.03 0.03

[0058] Samples were taken from the track steel prepared in Examples 1-3, and the terminal hardenability was tested according to GB / T 225, with a normalizing temperature of 900±10°C, a normalizing holding time of 30-35min, and a quenching temperature of 870±5°C. The terminal hardenability J25 and J30 indicators of the track shoes of the prior art and the present invention were tested respectively. The terminal hardenability data of the track shoes of the present invention and the prior art are shown in Table 4.

[0059] Table 4 Hardenability data of track shoe end of Example 1-3

[0060]

[0061] As shown in Table 4, compared with the track shoes prepared by the prior art, the track steel end hardenability after heat treatment of the present invention is improved, especially the J30 value is significantly improved, which confirms the improvement effect of the present invention on the hardenability of the track shoes. The teeth of the single-tooth track shoes for large bulldozers are thick and high (the maximum thickness can reach 60mm and the highest can reach 120mm). Limited by the hardening capacity of the existing technical steel, the hardness of the teeth decreases rapidly from the surface to the core after quenching, and the wear resistance is insufficient, which affects the service life of the track shoes. The present invention improves the J25 and J30 values, so that the track shoes of the largest specifications can reach a higher hardness from the surface to the core after heat treatment, thereby improving the wear resistance of the track shoes.

[0062] In winter when the ambient temperature is low (below 0°C), the microstructures of the track shoes prepared by the existing technology and the present invention are analyzed respectively. Figure 2 , Figure 3 and Figure 4 .from Figure 2 It can be seen that the metallographic structure of the track shoe produced in winter using the existing technology is a ferrite + pearlite matrix with a large amount of bainite distributed on it. As a brittle phase, the presence of bainite will cause the track shoe to crack during punching and shearing. Figure 3 It can be seen that the metallographic structure of the track plate produced in winter by the technology of the present invention is all ferrite + pearlite, without bainite structure. Due to the implementation of the end electromagnetic stirring and slow cooling technology of the ingot, the extreme difference of C, Mn and Cr is reduced, and the segregation degree is significantly reduced. Figure 4 It can be seen that even the center part of the track shoe is entirely composed of ferrite + pearlite structure, without bainite, which can meet the needs of punching and shearing processing.

[0063] The process parameters (such as temperature, time, etc.) of the present invention can realize the method by taking upper and lower limits and interval values, and the embodiments are not listed one by one here.

[0064] Any contents not described in detail in the present invention can be based on the conventional technical knowledge in the art.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.

Claims

1. A track shoe for a large bulldozer, characterized in that: The weight percentage of the chemical composition of the crawler shoe for large bulldozer is: C: 0.25-0.31%, Si: 0.36-0.80%, Mn: 1.15-1.30%, P≤0.015%, S≤0.010%, Cr: 0.70-0.90%, B: 0.0015-0.0030%, Ti: 0.025-0.055%, Al: 0.02-0.05%, N: 0.003-0.006%, H≤0.0002%, O≤0.0025%, As≤0.0080%, and the rest is iron and trace impurities. The extreme difference of C in the same cross section is ≤0.03%, the extreme difference of Mn is ≤0.04%, and the extreme difference of Cr is ≤0.05%.

2. The track shoe for a large bulldozer according to claim 1, characterized in that: The chemical composition weight percentage of the crawler plate for large bulldozer is: C: 0.26-0.29%, Si: 0.40-0.70%, Mn: 1.15-1.25%, P≤0.013%, S≤0.008%, Cr: 0.75-0.85%, B: 0.0015-0.0025%, Ti: 0.03-0.05%, Al: 0.02-0.04%, N: 0.003-0.005%, H≤0.0002%, O≤0.0020%, As≤0.0080%, and the rest is iron and trace impurities. The extreme difference of C in the same cross section is ≤0.02%, the extreme difference of Mn is ≤0.03%, and the extreme difference of Cr is ≤0.04%.

3. The track shoe for a large bulldozer according to claim 1, characterized in that: The track shoe hardenability value is 40HRC <J25≤45HRC,36HRC<J30≤42HRC。 4. The track shoe for a large bulldozer according to claim 1, characterized in that: The track shoe has a width of 300-400 mm, a tooth heel equivalent thickness of 40-60 mm, a tooth height of 85-120 mm, and a web thickness of 20-40 mm.

5. The track shoe for a large bulldozer according to claim 1, characterized in that: In winter when the ambient temperature is below 0°C, the metallographic structure of the track shoe obtained by natural cooling after hot rolling is all ferrite + pearlite.

6. A method for preparing a track shoe for a large bulldozer, comprising the following steps: Step S1: using low-As molten iron and scrap steel for converter smelting and LF+vacuum refining, the As content in the molten iron is ≤80ppm, and the molten iron accounts for no less than 80% of the raw materials for converter steelmaking; Step S2: using a continuous casting machine to cast a steel billet, the continuous casting machine is provided with an end electromagnetic stirring, the current is 450A-600A, and the straightening roll of the continuous casting machine is provided with a pressing function, and the pressing amount is 5-15mm; Step S3: Slowly cooling the steel billet in a slow cooling pit; Step S4: The steel billet is heated, rolled and cooled to form a track shoe.

7. The preparation method according to claim 6, characterized in that: In step S3, the slow cooling pit is first baked, and after the pit wall temperature reaches 750°C, the high-temperature steel billets off the continuous casting line are placed in the slow cooling pit for slow cooling, and the slow cooling time is greater than 24 hours before the billets are taken out of the slow cooling pit.

8. The preparation method according to claim 6, characterized in that: In the step S4, the steel billet is rough-rolled in 9 to 13 passes in the rolling process.

9. The preparation method according to claim 8, characterized in that: In the rough rolling pass, there are 1 to 2 scale breaking passes to loosen and peel off the iron oxide scale on the surface of the rolled piece. After the scale breaking pass, a ≥90° steel turning operation is added to remove the loose and peeling iron oxide scale from the rolled piece.

10. The preparation method according to claim 6, characterized in that: In step S4, the final rolling temperature is 940-1000°C.

Citation Information

Patent Citations

  • Carbon-manganese composite microalloyed steel for engineering machinery and preparation method thereof

    CN101654761A

  • Steel for low-carbon wear-resistant engineering machinery creeper tread and manufacturing method thereof

    CN101660101A

  • HB600 grade wear-resistant non-quenched and tempered steel plate and making method thereof

    CN104831189A

  • HB500-grade non-quenched and tempered wear-resisting steel plate and manufacturing method thereof

    CN106756565A

  • High-hardenability profile steel for ultra-large engineering machinery track and production method of high-hardenability profile steel