Method for preparing high-temperature corrosion-resistant coating based on low-temperature salt bath nitriding method, high-temperature corrosion-resistant coating and application

Through low-temperature salt bath nitriding method and pre-oxidation treatment, the problem of high energy consumption and serious pollution at high temperatures is solved, and a high-temperature corrosion-resistant coating is formed, which extends the service life of the workpiece and improves corrosion resistance. and antioxidant properties.

CN118910540APending Publication Date: 2024-11-08HUANENG HUNAN YUEYANG POWER GENERATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975868.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing salt bath nitriding method is carried out at high temperatures, resulting in high energy consumption, serious pollution and poor coating stability, affecting the service life of the workpiece.

Method used

The low-temperature salt bath nitriding method is used to preheat the workpiece and salt bath nitriding is performed at 400-500°C for 6 to 12 hours, and then pre-oxidation is performed to form a nitrogen-rich high-temperature corrosion-resistant coating. The raw materials of salt bath include sodium and potassium salts. The melting point of molten salt is reduced through aging oxidation treatment and the volatility of toxic pollutants is reduced.

Benefits of technology

The temperature of salt bath nitriding is reduced, environmental pollution is reduced, and the microstructure of the coating is uniformized through pre-oxidation treatment, which extends the service life of the workpiece, and improves corrosion resistance and oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910540A_ABST
    Figure CN118910540A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method, the high-temperature corrosion-resistant coating and application, and belongs to the technical field of material surface coatings. The method comprises the following steps: preheating a workpiece; the preheated workpiece is buried in a salt bath raw material, salt bath nitriding treatment is conducted for 6-12 h at the temperature of 400-500 DEG C, and a nitrogen-rich high-temperature corrosion-resistant coating is formed on the surface of the workpiece; and the nitrogen-rich high-temperature corrosion-resistant coating is subjected to pre-oxidation treatment, and the high-temperature corrosion-resistant coating is obtained. According to the method, the salt bath nitriding temperature is low, environmental pollution is reduced, the nitrogen-rich coating is subjected to pre-oxidation treatment, the microstructure of the coating is homogenized, internal residual stress is eliminated, the oxidation time of a workpiece in the using process is prolonged, then the service life of the workpiece is prolonged, and the prepared metal coating is good in surface quality, high in production efficiency and suitable for industrial production. And meanwhile, corrosion resistance and oxidation resistance are excellent, and the alloy is suitable for various metal parts such as carbon steel, austenitic steel and high-temperature alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material surface coatings, and specifically relates to a method for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method, a high-temperature corrosion-resistant coating and an application thereof. Background Art

[0002] After being used for a period of time, various workpieces will experience varying degrees of wear and corrosion, which will affect the work efficiency and service life of the workpieces. To address this, the current main method is to repair the surface of the workpiece to enhance the corrosion and wear resistance of the workpiece surface. Among them, different repair methods can be selected according to the type of coating and the shape of the substrate, such as slurry method (chroming, aluminum, silicon), salt bath method (nitriding) and embedding method (aluminum, titanium), etc.

[0003] Taking the salt bath method as an example, the salt bath nitriding method usually involves placing the workpiece in molten salt and forming a nitriding layer through high temperature insulation. The salt bath nitriding method has a simple process flow for preparing coatings, simple equipment investment, and low production cost. Due to the fluidity and temperature uniformity of the molten salt, the uniformity of the workpiece processing quality is greatly guaranteed; since the salt bath method is simple to operate, its processing objects can include most steel parts that have no special requirements for matrix strength.

[0004] However, due to the high-temperature volatilization characteristics of molten salt, the salt bath nitriding method needs to be carried out at a higher temperature.

[0005] For example, 560-580℃, etc., most of them need to be carried out at a temperature higher than 500℃, which consumes a lot of energy.

[0006] Moreover, at high temperatures, salt bath melting volatilizes toxic pollutants, which will pollute production conditions and go against green and environmentally friendly production requirements. In addition, the obtained coating has poor stability and will go through three stages during use: rapid oxidation, slow oxidation, and oxide layer peeling. During the rapid oxidation process, due to the oxidation rate problem, the coating structure will be unstable, thus affecting the use of the coating. The coating will be rapidly oxidized, shortening its service life. Summary of the invention

[0007] The present disclosure aims to solve at least one of the technical problems existing in the prior art, and provides a method for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method, a high-temperature corrosion-resistant coating and an application thereof.

[0008] In one aspect of the present disclosure, a method for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method is provided, the method comprising:

[0009] Preheating the workpiece;

[0010] The preheated workpiece is buried in a salt bath raw material and subjected to a salt bath nitriding treatment at 400-500°C for 6-12 hours to form a nitrogen-rich, high-temperature, corrosion-resistant coating on the surface of the workpiece;

[0011] The nitrogen-rich high-temperature corrosion-resistant coating is subjected to a pre-oxidation treatment to obtain a high-temperature corrosion-resistant coating.

[0012] Optionally, the salt bath raw materials include 40-50% sodium salt and 50-60% potassium salt.

[0013] Optionally, the sodium salt includes 28-35% sodium cyanide, 2-5% sodium carbonate and 10-20% sodium cyanate.

[0014] Optionally, the potassium salt includes 35-40% potassium cyanide, 2-5% potassium carbonate and 10-20% potassium cyanate.

[0015] Optionally, in the salt bath raw material, the content of cyanate is 15-30%.

[0016] Optionally, before the nitriding treatment, the salt bath raw material is subjected to an aging oxidation treatment at a temperature range of 500 to 650° C. for 12 to 24 hours.

[0017] Optionally, the preheating temperature is 200-240° C., and the preheating time is 30-60 min.

[0018] Optionally, the pre-oxidation treatment temperature is 80 to 150° C., and the pre-oxidation treatment time is 2 to 6 hours.

[0019] Another aspect of the present disclosure provides a high temperature corrosion resistant coating, which is prepared by the method described above.

[0020] Another aspect of the present disclosure provides an application of a high-temperature corrosion-resistant coating, wherein the high-temperature corrosion-resistant coating described above is applied to the surface of carbon steel, austenitic steel and high-temperature alloy.

[0021] The present disclosure provides a method for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method, a high-temperature corrosion-resistant coating and an application thereof, the method comprising: preheating a workpiece; burying the preheated workpiece in a salt bath raw material, performing a salt bath nitriding treatment at 400 to 500°C for 6 to 12 hours, and forming a nitrogen-rich high-temperature corrosion-resistant coating on the surface of the workpiece; and pre-oxidizing the nitrogen-rich high-temperature corrosion-resistant coating to obtain a high-temperature corrosion-resistant coating. The salt bath nitriding temperature of the method is low, which reduces environmental pollution. By pre-oxidizing the nitrogen-rich coating, the microstructure of the coating is homogenized, the internal residual stress is eliminated, and the oxidation time of the workpiece during use is extended, thereby increasing the service life of the workpiece. The formed coating is suitable for various metal parts such as carbon steel, austenitic steel and high-temperature alloys, and the prepared metal coating has good surface quality and high production efficiency, and has excellent corrosion resistance and oxidation resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a flowchart of a method for preparing a high-temperature corrosion-resistant coating according to an embodiment of the present disclosure;

[0023] Figure 2 This is a microscopic morphology photograph of the cross section of the high-temperature corrosion-resistant coating of Example 2 of the present disclosure. DETAILED DESCRIPTION

[0024] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0025] like Figure 1 As shown, in one aspect of the present disclosure, a method S100 for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method is provided, which specifically includes the following steps S110 to S130:

[0026] S110, preheating the workpiece.

[0027] In some preferred embodiments, the temperature of the workpiece preheating treatment is 200-240° C., and the preheating time is 30-60 min, so as to remove moisture from the workpiece surface and simultaneously heat the workpiece to meet the process requirements of the subsequent salt bath treatment.

[0028] As a further preferred embodiment, the temperature of the preheat treatment can be 200°C, 210°C, 220°C, 230°C, 240°C, and the time of the preheat treatment can be 30 min, 40 min, 50 min, 60 min.

[0029] It should be understood that before the preheat treatment of the workpiece, the surface of the workpiece may also be cleaned. For example, oil stains, dust, etc. on the surface of the workpiece may be cleaned with reagents such as alcohol or acetone, and oxides on the surface of the workpiece may be removed with a steel brush to improve surface cleanliness and enhance the nitriding effect.

[0030] S120, burying the preheated workpiece in a salt bath raw material, performing salt bath nitriding treatment at 400-500°C for 6-12 hours, and forming a nitrogen-rich, high-temperature, corrosion-resistant coating on the surface of the workpiece.

[0031] In some preferred embodiments, the temperature of the salt bath nitriding treatment is 400° C., 420° C., 450° C., 470° C., or 500° C., and the time is 6 h, 8 h, 10 h, or 12 h.

[0032] In other preferred embodiments, the salt bath raw materials include 40-50% sodium salt and 50-60% potassium salt.

[0033] As a further preferred embodiment, the sodium salt includes 28-35% sodium cyanide, 2-5% sodium carbonate and 10-20% sodium cyanate.

[0034] As a further preferred embodiment, the potassium salt includes 35-40% potassium cyanide, 2-5% potassium carbonate and 10-20% potassium cyanate.

[0035] It should be noted that the content of cyanate is 15-30%, that is, when the sodium salt includes sodium cyanate and the potassium salt includes potassium cyanate, sodium cyanate and potassium cyanate can be used as nitriding sources only when the total content of cyanate of the two is between 15-30%.

[0036] In this embodiment, the sodium cyanide and potassium cyanide treated by aging oxidation can provide sufficient CNO required for nitriding during the salt bath nitriding process at 400-500°C. - In addition, since the melting points of sodium cyanide and potassium cyanide are much lower than those of traditional nitriding molten salt components, the nitriding molten salt components can still have good fluidity at lower temperatures, ultimately achieving the purpose of low-temperature nitriding and reducing the adverse effects of the high-temperature and long-term nitriding process on the substrate.

[0037] It should be further explained that before step S120, the salt bath raw material is also subjected to oxidation treatment. For example, sodium salt and potassium salt are mixed to form a salt bath raw material, and the salt bath raw material is subjected to aging oxidation treatment at a temperature range of 500 to 650°C for 12 to 24 hours. During the aging oxidation treatment, sufficient reaction activation energy can be provided for the conversion of cyanide into cyanate. During the aging oxidation treatment at a temperature range of 500 to 650°C, part of the cyanide undergoes CN - +O2=2CNO - , CN -+CO2=CNO - +CO reaction to generate CNO - The reaction can continue in the subsequent 400-500℃ salt bath nitriding process, which not only meets the sufficient cyanate ion concentration required for nitriding, but also ensures that the salt bath raw materials are still mainly low-melting point salts and still have good fluidity at lower nitriding temperatures.

[0038] In some preferred embodiments, the salt bath raw material may be oxidized at 500° C., 550° C., 600° C., or 650° C. for 12 h, 15 h, 20 h, or 24 h.

[0039] In this embodiment, low-melting-point salts are selected and the component content is reasonably designed. At the same time, the low-temperature salt bath preparation of the nitriding coating is achieved by subjecting the prepared new salt to an aging oxidation treatment. At the same time, the temperature of the salt bath nitriding treatment is relatively low, and the volatility of the molten salt is reduced, which effectively reduces the volatilization of toxic pollutants and reduces pollution to the working environment.

[0040] S130, pre-oxidizing the nitrogen-rich high-temperature corrosion-resistant coating to obtain a high-temperature corrosion-resistant coating.

[0041] Specifically, the nitrogen-rich high-temperature corrosion-resistant coating sample obtained after salt bath nitriding is placed in a box-type resistance furnace, oxygen and carbon dioxide are introduced into it, and pre-oxidation treatment is performed at 80-150°C for 2-6 hours to obtain a high-temperature corrosion-resistant coating.

[0042] As a further preferred embodiment, the temperature of the pre-oxidation treatment is preferably 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C, and the time of the pre-oxidation treatment is preferably 2h, 3h, 4h, 5h, or 6h.

[0043] In this embodiment, a lower pre-oxidation treatment temperature can form Fe3O4 phase to promote nitriding while preventing the generation of Fe3O2 phase which is not conducive to the nitriding process. The pre-oxidation treatment can homogenize the microstructure of the coating, eliminate internal residual stress, increase stability, and extend the oxidation time of the workpiece during subsequent use, thereby extending the service life of the coating.

[0044] The preparation method disclosed in the present invention is simple and does not need to be carried out under atmosphere or vacuum conditions. At the same time, the nitriding layer preparation efficiency is high, and the thickness of the formed coating is adjustable within the range of 0.1 to 1.0 mm. It has good wear resistance and especially excellent resistance to high and low temperature corrosion and steam oxidation.

[0045] Another aspect of the present disclosure provides a high temperature corrosion resistant coating, which is prepared by the method described above. Please refer to the above description for the specific process, which will not be repeated here.

[0046] The high temperature corrosion resistant coating of this embodiment has a thickness of 0.1 to 1.0 mm. The coating within this thickness range has good wear resistance and corrosion resistance.

[0047] Another aspect of the present disclosure provides an application of a high-temperature corrosion-resistant coating, wherein the high-temperature corrosion-resistant coating described above is applied to the surface of carbon steel, austenitic steel and high-temperature alloy.

[0048] It should be noted that the present embodiment does not impose any specific restrictions on the types of workpieces to which the high-temperature corrosion-resistant coating can be applied, such as metal pipes, etc. It has a wide range of applications and is extremely practical.

[0049] The preparation method of the high temperature corrosion resistant coating will be further described below in conjunction with several specific embodiments:

[0050] Example 1

[0051] This example takes a large boiler pipe made of carbon steel as an example to prepare a high-temperature corrosion-resistant coating. The pipe specifications are all 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The steps are as follows:

[0052] S1. Pipeline surface cleaning

[0053] Use alcohol / acetone to clean oil stains, dust, etc. on the surface of the pipe, and use a steel brush to remove the surface oxide.

[0054] S2. Pipeline preheating treatment

[0055] The pipe was preheated at 220°C for 30 min.

[0056] S3, salt bath nitriding treatment

[0057] Under the condition of salt bath temperature of 400℃, the pipe was subjected to salt bath nitriding treatment for 6 hours.

[0058] Among them, the preparation method of the salt bath nitriding raw material is as follows: 35% of sodium cyanide, 3% of sodium carbonate and 12% of sodium cyanate are weighed by mass percentage, and mixed to obtain sodium salt; 35% of potassium cyanide, 2% of potassium carbonate and 13% of potassium cyanate are weighed by mass percentage, and mixed to obtain potassium salt; the prepared sodium salt and potassium salt are mixed and aged and oxidized at a temperature range of 500°C for 12 hours; when the cyanate content is 25%, it can be put into use.

[0059] S4. Pre-oxidation treatment

[0060] The inner surface coating of the workpiece was pre-oxidized at a temperature of 80°C and a time of 2 h.

[0061] The corrosion resistance of the coating was further tested in Example 1, as follows: In a 3.5 wt. % sodium chloride solution, the corrosion current density of the prepared nitrogen-rich coating sample was from 0.0296 mA / cm 2 (matrix) reduced to 0.0013586mA / cm 2 , the corrosion potential increases from -0.53V (substrate) to 0.28515V, and the corrosion resistance increases.

[0062] The wear resistance of the coating was further tested in Example 1, as follows: under the test conditions of a load of 10 g and a holding time of 10 s, the microhardness of the prepared nitrogen-rich coating was approximately 453 HV, and the microhardness of the carbon steel substrate was approximately 320 HV, and the hardness thereof was increased by about 1.4 times.

[0063] Example 2

[0064] This example takes a large boiler pipe made of austenitic steel as an example to prepare a high-temperature corrosion-resistant coating. The pipe specifications are all 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The steps are as follows:

[0065] S1. Pipeline surface cleaning

[0066] Use alcohol / acetone to clean oil stains, dust, etc. on the surface of the pipe, and use a steel brush to remove the surface oxide.

[0067] S2. Pipeline preheating treatment

[0068] The pipe was preheated at 220°C for 40 min.

[0069] S3, salt bath nitriding treatment

[0070] Under the condition of salt bath temperature of 450℃, the pipe was subjected to salt bath nitriding treatment for 6 hours.

[0071] Among them, the preparation method of salt bath nitriding raw materials is as follows: 35% sodium cyanide, 4% sodium carbonate and 11% sodium cyanate are weighed by mass percentage, and mixed to obtain sodium salt; 36% potassium cyanide, 3.2% potassium carbonate and 10.8% potassium cyanate are weighed by mass percentage, and mixed to obtain potassium salt; the prepared sodium salt and potassium salt are mixed and aged and oxidized at a temperature range of 500°C for 15 hours; when the cyanate content is 21.8%, it can be put into use.

[0072] S4. Pre-oxidation treatment

[0073] The inner surface coating of the workpiece was pre-oxidized at a temperature of 80°C and a time of 4 hours.

[0074] like Figure 2As shown, a layer of high-temperature corrosion-resistant nitriding coating with uniform and dense structure and metallurgical bonding with the alloy matrix is ​​obtained on the surface of the austenitic steel pipeline. The coating thickness is about 11.67μm and the N atomic content is about 8.68%. Tests show that the corrosion resistance and wear resistance of the coating sample are better than those of the base material sample.

[0075] In this Example 2, the corrosion resistance of the coating was further tested, as follows: In a 3.5wt.% sodium chloride solution, the corrosion current density of the prepared nitrogen-rich coating sample was from 0.00603mA / cm 2 (matrix) reduced to 0.00218mA / cm 2 , the corrosion potential increased from -0.69608V (substrate) to -0.26228V, and the corrosion resistance increased.

[0076] The wear resistance of the coating was further tested in Example 2, as follows: under the test conditions of a load of 10 g and a holding time of 10 s, the microhardness of the prepared nitrogen-rich coating was approximately 378 HV, and the microhardness of the austenitic steel substrate was approximately 190 HV, and its hardness was increased by about 2 times.

[0077] Example 3

[0078] This example takes a large boiler pipe made of high-temperature alloy as an example to prepare a high-temperature corrosion-resistant coating. The pipe specifications are all 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The steps are as follows:

[0079] S1. Pipeline surface cleaning

[0080] Use alcohol / acetone to clean oil stains, dust, etc. on the surface of the pipe, and use a steel brush to remove the surface oxide.

[0081] S2. Pipeline preheating treatment

[0082] The pipe was preheated at 220°C for 40 min.

[0083] S3, salt bath nitriding treatment

[0084] Under the condition of salt bath temperature of 450℃, the pipe was subjected to salt bath nitriding treatment for 6 hours.

[0085] Among them, the preparation method of salt bath nitriding raw materials is as follows: 30% sodium cyanide, 4% sodium carbonate and 12% sodium cyanate are weighed by mass percentage, and mixed to obtain sodium salt; 40% potassium cyanide, 3.2% potassium carbonate and 10.8% potassium cyanate are weighed by mass percentage, and mixed to obtain potassium salt; the prepared sodium salt and potassium salt are mixed and aged and oxidized at a temperature range of 550°C for 15 hours; when the cyanate content is 22.8%, it can be put into use.

[0086] S4. Pre-oxidation treatment

[0087] The inner surface coating of the workpiece was pre-oxidized at a temperature of 120°C and for 4 hours.

[0088] In this Example 3, the corrosion resistance of the coating was further tested, as follows: In a 3.5wt.% sodium chloride solution, the corrosion current density of the prepared nitrogen-rich coating sample was from 0.01864mA / cm 2 (matrix) reduced to 0.006093mA / cm 2 , the corrosion potential increased from -0.319V (substrate) to -0.232V, and the corrosion resistance increased.

[0089] The wear resistance of the coating was further tested in Example 3, as follows: the microhardness of the prepared nitrogen-rich coating was about 543 HV, and the microhardness of the high-temperature alloy substrate was about 300 HV, and the hardness thereof was increased by about 1.8 times.

[0090] The present disclosure provides a high-temperature corrosion-resistant coating and a preparation method and application thereof, which have the following beneficial effects compared with the prior art:

[0091] First, the preparation method of the nitrogen-rich high-temperature corrosion-resistant coating disclosed in the present invention does not need to be carried out under atmosphere or vacuum conditions, and the preparation process is simple. At the same time, the nitrogen-diffused layer has high preparation efficiency, adjustable thickness, good wear resistance, and especially excellent resistance to high and low temperature corrosion and steam oxidation.

[0092] Second, the salt bath nitriding temperature of the present disclosure is low, the volatility of the molten salt is reduced, and the pollution to the working environment is reduced;

[0093] Third, the nitrogen-rich high-temperature corrosion-resistant coating disclosed in the present invention is pre-oxidized to make the microstructure of the coating uniform, eliminate the internal residual stress, and increase the oxidation time of the workpiece in the subsequent use process, thereby extending the coating life;

[0094] Fourth, the nitrogen-rich high-temperature corrosion-resistant coating disclosed in the present invention is suitable for various types of metal workpieces whose surfaces need to be strengthened, including carbon steel, austenitic stainless steel, high-temperature alloys and other workpieces. It has a wide range of applications and is extremely practical.

[0095] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for preparing a high-temperature corrosion-resistant coating based on a low-temperature salt bath nitriding method, characterized in that: The method comprises: Preheating the workpiece; The preheated workpiece is buried in a salt bath raw material and subjected to a salt bath nitriding treatment at 400-500°C for 6-12 hours to form a nitrogen-rich, high-temperature, corrosion-resistant coating on the surface of the workpiece; The nitrogen-rich high-temperature corrosion-resistant coating is subjected to a pre-oxidation treatment to obtain a high-temperature corrosion-resistant coating.

2. The method according to claim 1, characterized in that The salt bath raw materials include 40-50% of sodium salt and 50-60% of potassium salt.

3. The method according to claim 2, characterized in that The sodium salt comprises 28-35% of sodium cyanide, 2-5% of sodium carbonate and 10-20% of sodium cyanate.

4. The method according to claim 3, characterized in that: The potassium salt comprises 35-40% of potassium cyanide, 2-5% of potassium carbonate and 10-20% of potassium cyanate.

5. The method according to claim 4, characterized in that In the salt bath raw material, the content of cyanate is 15-30%.

6. The method according to any one of claims 1 to 5, characterized in that: Before nitriding treatment, the salt bath raw materials are subjected to aging oxidation treatment at a temperature range of 500 to 650°C for 12 to 24 hours.

7. The method according to any one of claims 1 to 5, characterized in that: The preheating temperature is 200-240° C., and the preheating time is 30-60 minutes.

8. The method according to any one of claims 1 to 5, characterized in that: The temperature of the pre-oxidation treatment is 80-150° C., and the time of the pre-oxidation treatment is 2-6 hours.

9. A high temperature corrosion resistant coating, characterized in that: The method according to any one of claims 1 to 8 is used to prepare the product.

10. An application of a high temperature corrosion resistant coating, characterized in that: The high temperature corrosion resistant coating described in claim 9 is applied to the surface of carbon steel, austenitic steel and high temperature alloy.