Preparation method of metal cobalt film and silicide thereof
The electrical performance damage of metal cobalt film deposition in the prior art was solved by pretreatment and pulsed atomic layer deposition technology, and the cobalt silicide was formed in the prior art. and shadow effect problems, high-quality cobalt film and cobalt silicide preparation are achieved, meeting the application needs of new devices.
Patent Information
- Application Number
- CN202410986240.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art has electrical performance damage and shadowing effects when depositing metal cobalt films, making it difficult to achieve conformal deposition in three-dimensional structures and cannot meet the application needs of modern logic and dynamic random access memory.
The pretreated silicon-based three-dimensional substrate is used to form a cobalt buffer layer and a metal cobalt film in different reaction chambers by pulsed atomic layer deposition method, and cobalt silicide is formed in combination with titanium nitride annealing, and the multi-cavity atomic layer deposition equipment is simplified. Process and reduce costs.
A high-quality metal cobalt film preparation has been achieved, with a cobalt content of more than 90%, an appropriate resistivity, and a cobalt metal silicide suitable for new devices is formed through annealing to meet the application needs of the device.
Smart Images

Figure CN118910580A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal film preparation, and in particular to a method for preparing a metal cobalt film and its silicide. Background Art
[0002] As semiconductor devices continue to shrink, contact resistance is considered to be one of the important parasitic elements that determine the overall performance of the device. In modern logic and dynamic random access memory (DRAM) technology, the contact points are located in three-dimensional deep contact holes with high aspect ratios, which is particularly problematic for depositing metals used to form contacts in deep contact holes. Since physical vapor deposition (PVD) has certain limitations in terms of conformality, a new thin film deposition process is needed.
[0003] Atomic layer deposition (ALD) is a method that can deposit materials layer by layer on the surface of a substrate in the form of a single atomic film. However, compared with oxide or nitride ALD, the metal ALD process is relatively difficult, especially the ALD preparation of transition metals. At present, although plasma-enhanced CVD or ALD can be used to deposit metal Co films, the plasma in the plasma-enhanced method will cause electrical damage to the device. In addition, the plasma also has a shadow effect on the three-dimensional structure, and conformal deposition cannot be achieved, so it cannot meet the application requirements of the device well.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a metal cobalt thin film and its silicide, which can well meet the application requirements of new devices.
[0006] The present invention provides a method for preparing a metal cobalt thin film, comprising the following steps:
[0007] S1: pre-treating a silicon-based three-dimensional substrate to obtain a pre-treated silicon-based three-dimensional substrate;
[0008] S2: placing the pretreated silicon-based three-dimensional substrate in a first reaction chamber, using a first gas as a carrier gas, sequentially pulsing a first cobalt precursor and a first reaction gas to perform a first atomic layer deposition, and forming a cobalt buffer layer on the pretreated silicon-based three-dimensional substrate;
[0009] S3: placing a pretreated silicon-based three-dimensional substrate on which a cobalt buffer layer is formed in a second reaction chamber, using a second gas as a carrier gas, and sequentially pulsing a second cobalt precursor and a second reaction gas to perform a second atomic layer deposition to form a metal cobalt film on the cobalt buffer layer.
[0010] In step S1, the pretreatment includes wet treatment, which is mainly used to remove the oxide layer on the silicon-based three-dimensional substrate; specifically, the wet treatment is carried out using a mixed solution of water and dihydrofuran (DHF), the volume ratio of water to dihydrofuran in the mixed solution is 100: (0.5-1.5), and the wet treatment time is 30s-2min.
[0011] Furthermore, the pretreatment also includes a degassing treatment, a pre-cleaning treatment and a heat treatment performed in sequence; wherein the degassing treatment method is lamp irradiation or base heating, the base heating temperature is 240-260°C, and the base heating time is 25-35s; the pre-cleaning treatment is performed using a remote plasma mixed gas of NF3 and NH3, the volume ratio of NF3 to NH3 in the remote plasma mixed gas is 1:(0.8-1.2), the pre-cleaning treatment time is 15-25s, and the pre-cleaning treatment can be performed under radio frequency conditions, the radio frequency power is 20-40W, and the radio frequency frequency is 40-100KHz; the heat treatment temperature is 170-190°C, the heat treatment time is 15s-2min, and the heat treatment is mainly used to remove the natural oxide layer on the surface.
[0012] In step S2, the temperature of the first reaction chamber is 150-200°C; the first gas is argon; the first cobalt precursor is bis(N,N'-di-iso-propylacetamidine)cobalt(II), and the temperature of the first cobalt precursor is 60-70°C; the pulse time of the first cobalt precursor is 0.5-2s, and the first cobalt precursor is vacuumed for 0.2-3s after pulsing.
[0013] Furthermore, the first reaction gas is a remote plasma of hydrogen or hydrogen; the pulse time of the first reaction gas is 0.5-5s; the first atomic layer deposition is carried out under RF conditions, the RF power is 30-200W, and the RF frequency is 40-100KHz; the vacuum is drawn for 0.5-3s after the pulse of the first reaction gas; the thickness of the cobalt buffer layer is 0.5-1.5nm.
[0014] In step S3, the temperature of the second reaction chamber is 250-320°C; the second gas is argon; the second cobalt precursor is bis(N,N'-di-iso-propylacetamidine)cobalt(II), and the temperature of the second cobalt precursor is 60-70°C; the pulse time of the second cobalt precursor is 0.5-2s, and the vacuum is evacuated for 0.2-3s after pulsing the second cobalt precursor.
[0015] Furthermore, the second reaction gas is hydrogen or ammonia; the pulse time of the second reaction gas is 0.5-5s; vacuum is drawn for 0.5-2s after the pulse of the second reaction gas; and the thickness of the metal cobalt film is 8-30nm.
[0016] The present invention also provides a method for preparing a metal cobalt thin film silicide, comprising the following steps:
[0017] A) preparing a metal cobalt thin film by using the above preparation method;
[0018] B) After titanium nitride is deposited on the surface of the metal cobalt film, annealing and cleaning are performed.
[0019] In step B), titanium nitride is deposited by PVD, MOCVD or thermal ALD; the thickness of titanium nitride is 2-10nm; the annealing temperature is 800-950℃, and the annealing time is 25-35s; the cleaning includes a first cleaning and a second cleaning performed in sequence; wherein the first cleaning is performed by a mixed solution of NH4OH, H2O2 and H2O, the volume ratio of NH4OH, H2O2 and H2O in the mixed solution is 1:(0.8-1.2):(4-6), the first cleaning temperature is 40-60℃, and the first cleaning time is 5-10min; the second cleaning is performed by a mixed solution of H3PO4, HNO3 and CH3COOH, the volume ratio of H3PO4, HNO3 and CH3COOH in the mixed solution is 70:(1-3):(10-15), the second cleaning temperature is 70-80℃, and the second cleaning time is 15-25min.
[0020] The preparation method of the present invention can be carried out by conventional atomic layer deposition equipment, and each step can be carried out in the same cavity or in different cavities; specifically, it can be carried out by multi-cavity atomic layer deposition equipment, which includes a transmission cavity and multiple cavities spaced outside the transmission cavity, and the multiple cavities can be reasonably configured according to actual needs. The multiple cavities are respectively connected to the transmission cavity, and a transmission arm is provided in the transmission cavity. The transmission arm can transfer the substrate between the transmission cavity and the multiple cavities so that the substrate can carry out each step in the multiple cavities. The multiple cavities can include a degassing cavity, a pre-cleaning cavity, a first reaction cavity, a second reaction cavity, and a titanium nitride deposition cavity, which are respectively used for the above-mentioned degassing treatment, pre-cleaning treatment, first atomic layer deposition, second atomic layer deposition, and titanium nitride deposition. The preparation of metal cobalt thin films and silicides thereof by multi-cavity atomic layer deposition equipment greatly reduces production costs, simplifies production processes, and improves production efficiency.
[0021] The cobalt content in the metal cobalt film prepared by the present invention exceeds 90%, and the resistivity of the metal cobalt film reaches about 20 μohm·cm. Cobalt metal silicide can be formed after annealing, which can well meet the application requirements of new devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 This is an electron microscope image of the metal cobalt film prepared in Example 1;
[0024] Figure 2 This is the atomic content distribution diagram of the metal cobalt film prepared in Example 1;
[0025] Figure 3 This is an electron microscope image of the metal cobalt thin film silicide prepared in Example 3;
[0026] Figure 4 The XRD spectrum of the metal cobalt thin film silicide prepared in Example 3;
[0027] Figure 5 This is an electron microscope image of the metal cobalt film prepared in Comparative Example 1;
[0028] Figure 6 This is an electron microscope image of the metal cobalt thin film silicide prepared in Comparative Example 1. DETAILED DESCRIPTION
[0029] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment provides a method for preparing a metal cobalt thin film, the steps are as follows:
[0034] S1: Preprocessing
[0035] Firstly, the silicon-based three-dimensional substrate was wet-treated with a mixed solution of water and dihydrofuran (DHF), wherein the volume ratio of water to dihydrofuran in the mixed solution was 100:1 and the wet treatment time was 30 seconds to remove the oxide layer on the silicon-based three-dimensional substrate.
[0036] Subsequently, the silicon-based three-dimensional substrate was degassed by using a base heating method, and the base heating temperature was controlled to be 250°C and the base heating time was 30s.
[0037] Next, the silicon-based three-dimensional substrate was pre-cleaned using a remote plasma mixed gas of NF3 and NH3. The volume ratio of NF3 and NH3 in the remote plasma mixed gas was 1:1, the base temperature was controlled at 35°C, and the pre-cleaning time was 20s. The pre-cleaning treatment was carried out under RF conditions with an RF power of 30W and a RF frequency of 70KHz.
[0038] Finally, the silicon-based three-dimensional substrate is heat-treated, the heat treatment temperature is controlled to be 180°C, the heat treatment time is 1 min, the natural oxide layer on the surface is removed, and a pretreated silicon-based three-dimensional substrate is obtained.
[0039] S2: Preparation of cobalt buffer layer
[0040] The pretreated silicon-based three-dimensional substrate is transferred to the first reaction chamber in a vacuum environment, the temperature of the first reaction chamber is controlled to be 180°C, argon is used as a carrier gas, and then di(N,N'-di-iso-propylacetamidine)cobalt(II) with a temperature of 65°C is pulsed into the first reaction chamber in a pulsed manner, each pulse time is 1s, and vacuum is evacuated for 2s after the pulse; then, remote plasma of hydrogen is pulsed into the first reaction chamber in a pulsed manner, and atomic layer deposition is performed under radio frequency conditions, with an radio frequency power of 120W, a radio frequency frequency of 70KHz, each pulse time is 3s, and vacuum is evacuated for 2s after the pulse; the above steps are repeated for 6 cycles to form a cobalt buffer layer with a thickness of about 1nm on the pretreated silicon-based three-dimensional substrate.
[0041] S3: Preparation of metallic cobalt thin film
[0042] In a vacuum environment, a pretreated silicon-based three-dimensional substrate with a cobalt buffer layer formed thereon is transferred to a second reaction chamber, the temperature of the second reaction chamber is controlled to be 280°C, argon is used as a second carrier gas, and then di(N,N'-di-iso-propylacetamidine)cobalt(II) at a temperature of 65°C is pulsed into the second reaction chamber in a pulsed manner, each pulse lasting 1 second, and the chamber is evacuated for 2 seconds after the pulse; then, hydrogen is pulsed into the second reaction chamber in a pulsed manner for atomic layer deposition, each pulse lasting 3 seconds, and the chamber is evacuated for 1 second after the pulse; the above steps are repeated 466 times to form a metal cobalt film with a thickness of about 30 nm on the metal cobalt film.
[0043] The electron microscope image and atomic content distribution diagram of the metal cobalt film prepared in this example are shown in FIG. Figure 1 , Figure 2 As shown; the results show that the surface of the metal cobalt film is relatively flat and its main component is metal cobalt.
[0044] The cobalt content and resistivity of the metal cobalt film prepared in this embodiment were tested, and the results showed that the cobalt content of the metal cobalt film in this embodiment was 90%, and the resistivity was about 18 μohm·cm.
[0045] Example 2
[0046] Except that the above steps are repeated 155 times in step S3 to form a metal cobalt film with a thickness of about 8 nm on the metal cobalt film, the rest is the same as Example 1.
[0047] Example 3
[0048] This embodiment provides a method for preparing a metal cobalt thin film silicide, the steps of which are as follows:
[0049] 1) Preparation of metal cobalt thin film
[0050] The metal cobalt thin film was prepared by the methods of Examples 1 and 2 respectively.
[0051] 2) Preparation of metal cobalt thin film silicide
[0052] Titanium nitride was deposited on the metal cobalt film by thermal ALD method. The thermal ALD process was as follows: the base temperature of the equipment was 400°C, TiCL4 and NH3 were used as precursors, the TiCl4 source temperature was 21°C, the TiCl4 pulse was 0.3s, and the TiCl4 pipeline was pumped out for 2s; the NH3 pulse was 2s, and the NH3 pipeline was pumped out for 4s. The above process was repeated 240 times to form a titanium nitride layer with a thickness of 5nm on the metal cobalt film.
[0053] The pretreated silicon-based three-dimensional substrate deposited with a titanium nitride layer was annealed, and the annealing temperatures were set to 500° C., 700° C., 800° C., and 900° C., respectively, and the annealing time was 30 s.
[0054] The pretreated silicon-based three-dimensional substrate after annealing is cleaned, and the cleaning includes a first cleaning and a second cleaning performed in sequence; wherein the first cleaning is performed using a mixed solution of NH4OH, H2O2 and H2O, the volume ratio of NH4OH, H2O2 and H2O in the mixed solution is 1:1:5, the first cleaning temperature is 50°C, and the first cleaning time is 8 minutes; the second cleaning is performed using a mixed solution of H3PO4, HNO3 and CH3COOH, the volume ratio of H3PO4, HNO3 and CH3COOH in the mixed solution is 70:2:12, the second cleaning temperature is 75°C, and the second cleaning time is 20 minutes, and a metal cobalt thin film silicide is obtained after cleaning.
[0055] The electron microscope image of the metal cobalt thin film silicide prepared at an annealing temperature of 800°C is shown in Figure 3 As shown; the results show that a relatively flat cobalt metal silicide can be formed on a silicon substrate.
[0056] The XRD patterns of the metal cobalt thin film silicide prepared at annealing temperatures of 500°C, 700°C, 800°C, and 900°C are as follows: Figure 4 As shown; the results show that: CoSi silicide will not be formed at a low temperature of 500°C, and the metal cobalt film prepared by the above method directly forms Co2Si silicide above 700°C.
[0057] Example 4
[0058] This embodiment provides a method for preparing a metal cobalt thin film silicide, the steps of which are as follows:
[0059] S1: Preprocessing
[0060] The silicon-based three-dimensional substrate is pretreated by the method of Example 1 to obtain a pretreated silicon-based three-dimensional substrate.
[0061] S2: Preparation of cobalt buffer layer
[0062] The pretreated silicon-based three-dimensional substrate is transferred to a first reaction chamber in a vacuum environment, the temperature of the first reaction chamber is controlled to be 150°C, argon gas is pulsed into the first reaction chamber for protection, and then di(N,N'-di-iso-propylacetamidine)cobalt(II) at a temperature of 60°C is pulsed into the first reaction chamber in a pulsed manner, each pulse time is 0.5s, and vacuum is evacuated for 1s after the pulse; then, remote plasma of hydrogen is pulsed into the first reaction chamber in a pulsed manner, and atomic layer deposition is performed under radio frequency conditions, with an radio frequency power of 30W, a radio frequency frequency of 40KHz, each pulse time is 0.5s, and vacuum is evacuated for 1s after the pulse; the above steps are repeated for 2 cycles to form a cobalt buffer layer on the pretreated silicon-based three-dimensional substrate.
[0063] S3: Preparation of metallic cobalt thin film
[0064] In a vacuum environment, a pretreated silicon-based three-dimensional substrate with a cobalt buffer layer formed thereon is transferred to a second reaction chamber, the temperature of the second reaction chamber is controlled to be 250°C, argon gas is pulsed into the second reaction chamber for protection, and then di(N,N'-di-iso-propylacetamidine)cobalt(II) at a temperature of 60°C is pulsed into the second reaction chamber in a pulsed manner, each pulse time is 0.5s, and vacuum is evacuated for 1s after the pulse; then, ammonia gas is pulsed into the second reaction chamber in a pulsed manner for atomic layer deposition, each pulse time is 0.5s, and vacuum is evacuated for 0.5s after the pulse; the above steps are repeated 155 times to form a metal cobalt film on the metal cobalt film.
[0065] S4: Preparation of metal cobalt thin film silicide
[0066] Titanium nitride is deposited on the metal cobalt film by a thermal ALD method, so as to form a titanium nitride layer with a thickness of 5 nm on the metal cobalt film.
[0067] The pre-treated silicon-based three-dimensional substrate deposited with a titanium nitride layer was annealed, and the annealing temperature was set to 950° C. and the annealing time was 25 s.
[0068] The method of Example 3 is used to clean the pretreated silicon-based three-dimensional substrate after annealing to obtain a metal cobalt thin film silicide.
[0069] Example 5
[0070] This embodiment provides a method for preparing a metal cobalt thin film silicide, the steps of which are as follows:
[0071] S1: Preprocessing
[0072] The silicon-based three-dimensional substrate is pretreated by the method of Example 1 to obtain a pretreated silicon-based three-dimensional substrate.
[0073] S2: Preparation of cobalt buffer layer
[0074] The pretreated silicon-based three-dimensional substrate is transferred to the first reaction chamber in a vacuum environment, the temperature of the first reaction chamber is controlled to be 200°C, argon gas is pulsed into the first reaction chamber for protection, and then di(N,N'-di-iso-propylacetamidine)cobalt(II) at a temperature of 70°C is pulsed into the first reaction chamber in a pulsed manner, each pulse time is 2s, and vacuum is evacuated for 3s after the pulse; then, hydrogen is pulsed into the first reaction chamber in a pulsed manner, and atomic layer deposition is performed under radio frequency conditions, with an radio frequency power of 200W, a radio frequency frequency of 100KHz, each pulse time is 5s, and vacuum is evacuated for 3s after the pulse; the above steps are repeated 10 times to form a cobalt buffer layer on the pretreated silicon-based three-dimensional substrate.
[0075] S3: Preparation of metallic cobalt thin film
[0076] In a vacuum environment, a pretreated silicon-based three-dimensional substrate with a cobalt buffer layer formed thereon is transferred to a second reaction chamber, the temperature of the second reaction chamber is controlled to be 320°C, argon gas is pulsed into the second reaction chamber for protection, and then di(N,N'-di-iso-propylacetamidine)cobalt(II) at a temperature of 70°C is pulsed into the second reaction chamber in a pulsed manner, each pulse time is 2s, and vacuum is evacuated for 3s after the pulse; then, ammonia gas is pulsed into the second reaction chamber in a pulsed manner for atomic layer deposition, each pulse time is 5s, and vacuum is evacuated for 2s after the pulse; the above steps are repeated 155 times to form a metal cobalt film on the metal cobalt film.
[0077] S4: Preparation of metal cobalt thin film silicide
[0078] Titanium nitride is deposited on the metal cobalt film by a thermal ALD method, so as to form a titanium nitride layer with a thickness of 5 nm on the metal cobalt film.
[0079] The pre-treated silicon-based three-dimensional substrate deposited with titanium nitride was annealed, and the annealing temperature was set to 800° C. and the annealing time was set to 35 s.
[0080] The method of Example 3 is used to clean the pretreated silicon-based three-dimensional substrate after annealing to obtain a metal cobalt thin film silicide.
[0081] Comparative Example 1
[0082] In this comparative example, a conventional thermal ALD process is used to prepare a metal cobalt film with a thickness of about 30 nm on the pretreated silicon-based three-dimensional substrate of Example 1, and then a titanium nitride layer with a thickness of 5 nm is formed on the metal cobalt film using the method of Example 1.
[0083] The electron microscope images of the metal cobalt film and the metal cobalt film silicide prepared in this comparative example are as follows: Figure 5 , Figure 6 As shown; the results show that the surface of the metal cobalt film prepared in this comparative example is relatively rough, and a discontinuous cobalt metal silicide (such as Figure 6 shown).
[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a metal cobalt thin film, It is characterized in that The steps include: S1: pre-treating a silicon-based three-dimensional substrate to obtain a pre-treated silicon-based three-dimensional substrate; S2: placing the pretreated silicon-based three-dimensional substrate in a first reaction chamber, using a first gas as a carrier gas, sequentially pulsing a first cobalt precursor and a first reaction gas to perform a first atomic layer deposition, and forming a cobalt buffer layer on the pretreated silicon-based three-dimensional substrate; S3: placing a pretreated silicon-based three-dimensional substrate on which a cobalt buffer layer is formed in a second reaction chamber, using a second gas as a carrier gas, and sequentially pulsing a second cobalt precursor and a second reaction gas to perform a second atomic layer deposition to form a metal cobalt film on the cobalt buffer layer.
2. The preparation method according to claim 1, It is characterized in that In step S1, the pretreatment includes wet treatment; the wet treatment is carried out using a mixed solution of water and dihydrofuran, the volume ratio of water to dihydrofuran in the mixed solution is 100:(0.5-1.5), and the wet treatment time is 30s-2min.
3. The preparation method according to claim 2, It is characterized in that The pretreatment also includes degassing, pre-cleaning and heat treatment in sequence; the degassing method is lamp irradiation or base heating, the base heating temperature is 240-260℃, and the base heating time is 25-35s; the pre-cleaning method uses NF 3 With NH 3 The remote plasma mixed gas is used for the NF 3 With NH 3 The volume ratio is 1:(0.8-1.2), the pre-cleaning treatment time is 15-25s, the pre-cleaning treatment is carried out under radio frequency conditions, the radio frequency power is 20-40W, the radio frequency frequency is 40-100KHz; the heat treatment temperature is 170-190℃, and the heat treatment time is 15s-2min.
4. The preparation method according to claim 1, It is characterized in that In step S2, the temperature of the first reaction chamber is 150-200°C; the first gas is argon; the first cobalt precursor is bis(N,N'-di-iso-propylacetamidine)cobalt(II), and the temperature of the first cobalt precursor is 60-70°C; the pulse time of the first cobalt precursor is 0.5-2s, and the first cobalt precursor is vacuumed for 0.2-3s after pulsing.
5. The preparation method according to claim 4, It is characterized in that In step S2, the first reaction gas is a remote plasma of hydrogen or hydrogen; the pulse time of the first reaction gas is 0.5-5s; the first atomic layer deposition is performed under RF conditions, the RF power is 30-200W, and the RF frequency is 40-100KHz; the vacuum is drawn for 0.5-3s after pulsing the first reaction gas; the thickness of the cobalt buffer layer is 0.5-1.5nm.
6. The preparation method according to claim 1, It is characterized in that In step S3, the temperature of the second reaction chamber is 250-320°C; the second gas is argon; the second cobalt precursor is bis(N,N'-di-iso-propylacetamidine)cobalt(II), and the temperature of the second cobalt precursor is 60-70°C; the pulse time of the second cobalt precursor is 0.5-2s, and the vacuum is evacuated for 0.2-3s after pulsing the second cobalt precursor.
7. The preparation method according to claim 6, It is characterized in that In step S3, the second reaction gas is hydrogen or ammonia; the pulse time of the second reaction gas is 0.5-5s; vacuum is drawn for 0.5-2s after the second reaction gas is pulsed; and the thickness of the metal cobalt film is 8-30nm.
8. A method for preparing a metal cobalt thin film silicide, It is characterized in that The steps include: A) preparing a metal cobalt thin film by the preparation method according to any one of claims 1 to 7; B) After titanium nitride is deposited on the surface of the metal cobalt film, annealing and cleaning are performed.
9. The preparation method according to claim 8, It is characterized in that Titanium nitride is deposited by PVD, MOCVD or thermal ALD; the thickness of titanium nitride is 2-10nm; the annealing temperature is 800-950°C, and the annealing time is 25-35s.
10. The preparation method according to claim 8, It is characterized in that In step B), the cleaning includes a first cleaning and a second cleaning performed sequentially; wherein the first cleaning is performed using NH 4 OH, H 2 O 2 and H 2 O mixed solution, NH 4 OH, H 2 O 2 With H 2 The volume ratio of O is 1: (0.8-1.2): (4-6), the first cleaning temperature is 40-60 ° C, the first cleaning time is 5-10min; the second cleaning adopts H 3 PO 4 , HNO 3 and CH 3 The mixed solution of COOH was carried out, and H 3 PO 4 , HNO 3 With CH 3 The volume ratio of COOH is 70:(1-3):(10-15), the second cleaning temperature is 70-80°C, and the second cleaning time is 15-25 minutes.