RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction and preparation method of RuO2 / MoO3 composite nanowire electrocatalyst

Through the electrospinning and calcining method of RuO2/MoO3 composite nanowire electrocatalyst, the problem of insufficient stability of acid oxygen-evolution electrocatalysts is solved, and efficient catalytic performance and long-term stability under acidic conditions are achieved, which is significantly better than traditional RuO2 Nanowires.

CN118910669APending Publication Date: 2024-11-08RES & DEV INST OF NORTHWESTERN POLYTECHNICAL UNIV IN SHENZHEN
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411054644.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The lack of stability of existing acidic oxygen evolution electrocatalysts under acidic conditions leads to rapid attenuation of catalytic activity, making it difficult to work in highly oxidative and corrosive environments for a long time.

Method used

Using RuO2/MoO3 composite nanowire electrocatalyst, prepared by electrospinning and calcining, a nanowire structure with RuO2 and MoO3 nanoparticles stacked is formed. The molar ratio is 9:1 to 8:2, and the lattice oxygen of MoO3 is used instead of RuO2. lattice oxygen avoids excessive oxidation of RuO2 surface, thereby improving catalytic stability.

Benefits of technology

The performance of acidic electrocatalytic decomposition of water oxygen analysis is significantly improved. The oxygen evolution performance is better than that of commercial RuO2 and homemade RuO2 nanowires. It can work continuously in acidic electrolyte for 300 hours, inhibits Ru's dissolution and maintains high activity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910669A_ABST
    Figure CN118910669A_ABST
Patent Text Reader

Abstract

The invention discloses a RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction and a preparation method of the RuO2 / MoO3 composite nanowire electrocatalyst, and belongs to the technical field of catalytic material preparation. A RuO2 / MoO3 composite nanowire electrocatalyst for an acidic oxygen evolution reaction is characterized in that the electrocatalyst is a nanowire formed by stacking RuO2 and MoO3 nanoparticles, the diameter of the nanowire is 30-50nm, the length of the nanowire is 1-5mu m, and the molar ratio of RuO2 to MoO3 is (9: 1)-(8: 2). The preparation method of the electrocatalyst comprises the following steps: preparing electrostatic spinning sol; preparing nanofibers through electrostatic spinning; and preparing the RuO2 / MoO3 composite nanowire electrocatalyst. The novel electrocatalyst is provided for high-activity and high-stability acid oxygen evolution reaction, and the preparation method is simple, environmentally friendly, easy to control, capable of achieving large-scale production and high in applicability and can be popularized to preparation and large-scale production of other electrocatalytic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalytic material preparation, and in particular to a RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction and a preparation method thereof. Background Art

[0002] Electrocatalytic water hydrogen production plays a vital role in renewable energy utilization and storage technology. However, among the many water electrolysis technologies, proton exchange membrane water electrolyzer (PEMWE) has many advantages in overall water separation, such as higher mass transfer rate, product purity and reaction efficiency, and has more prospects in practical applications. Due to the slow kinetics of oxygen evolution reaction, it is an important goal to develop efficient oxygen evolution electrocatalysts to reduce the reaction energy barrier, promote the reaction and reduce energy consumption. Although a large number of efficient and stable alkaline catalysts have been developed, the development of acidic oxygen evolution reaction catalysts has not met expectations. In particular, due to the highly oxidizing and corrosive environment, the life of most oxygen evolution electrocatalysts under acidic conditions is a huge challenge. Therefore, it is challenging and important to develop efficient and stable oxygen evolution electrocatalysts in acidic media.

[0003] As the cheapest platinum group metal element ruthenium, ruthenium oxide has a more suitable binding energy for oxygen-containing intermediates and exhibits higher activity, showing great potential to replace iridium oxide as a PEMWE anode catalyst. Although ruthenium oxide has excellent catalytic activity, its catalytic stability is seriously insufficient due to the dissolution caused by excessive oxidation of ruthenium. Therefore, it is of great significance to synthesize ruthenium oxide-based composite electrocatalysts and improve their stability through a simple and effective method. Summary of the invention

[0004] The technical problem to be solved by the present invention is to address the deficiencies of the above-mentioned prior art and to propose a RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction and a preparation method thereof.

[0005] To achieve its purpose, the present invention adopts the following technical solutions:

[0006] A RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction, wherein the electrocatalyst is a nanowire formed by stacking RuO2 and MoO3 nanoparticles, wherein the nanowire has a diameter of 30 to 50 nm and a length of 1 to 5 μm, wherein the molar ratio of RuO2 to MoO3 is 9:1 to 8:2.

[0007] Preferably, in the electrocatalyst, the molar ratio of RuO2 to MoO3 is 8.5:1.5.

[0008] The present invention also aims to provide a method for preparing a RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction, which specifically comprises the following steps:

[0009] Step 1: Preparation of electrospinning sol:

[0010] Dissolving polyvinyl pyrrolidone and ruthenium trichloride in N,N-dimethylformamide respectively, dissolving ammonium molybdate in deionized water, then dropping the ruthenium trichloride solution into the polyvinyl pyrrolidone solution, stirring for 4 to 8 hours, then dropping the ammonium molybdate solution, stirring for 8 to 12 hours, to obtain an electrospinning sol;

[0011] Step 2: Electrospinning to prepare nanofibers:

[0012] After the electrospinning sol was allowed to stand for 1 to 2 hours, it was placed in a syringe and electrospun into nanofibers using an electrospinning system;

[0013] Step 3: Preparation of RuO2 / MoO3 composite nanowire electrocatalyst:

[0014] The nanofibers are exposed to air for 20 to 24 hours, then transferred to a quartz tube, calcined at 200 to 500° C. for 4 to 8 hours in an air atmosphere, and cooled to room temperature to obtain a RuO2 / MoO3 composite nanowire electrocatalyst.

[0015] Preferably, in step 1, the concentration of polyvinyl pyrrolidone in the electrospinning sol is 100-200 mg / mL, the concentration of ruthenium trichloride is 10-30 mg / mL, the concentration of ammonium molybdate is 1-10 mg / mL, and the volume ratio of N,N-dimethylformamide to deionized water is 2:1-6:1.

[0016] Further preferably, in step 1, the concentration of polyvinyl pyrrolidone in the electrospinning sol is 130-150 mg / mL, the concentration of ruthenium trichloride is 20-25 mg / mL, the concentration of ammonium molybdate is 2-4 mg / mL, and the volume ratio of N,N-dimethylformamide to deionized water is 4:1-5:1.

[0017] Preferably, in step 2, the electrospinning sol is ejected from a syringe pump at a flow rate of 1 to 10 μL / min using an electrospinning system, the distance between the metal needle and the aluminum foil is fixed at 15 to 20 cm, and the external magnetic field is 10 to 14 kV.

[0018] Preferably, in step 3, calcination is performed at 350° C. in an air atmosphere for 5 to 8 hours.

[0019] Preferably, in step 3, the heating rate of the calcination is 2-5°C / min.

[0020] Beneficial effects of the present invention:

[0021] 1. The present invention synthesizes binary RuO2 / MoO3 composite nanowires by a simple electrospinning / calcination method. The nanowires are formed by stacking RuO2 and MoO3 nanoparticles, so they have a large number of heterojunction interfaces, which significantly improves the performance of acidic electrocatalytic water decomposition and oxygen evolution. The oxygen evolution performance is much better than that of commercial RuO2 and homemade RuO2 nanowires, and the current density at 1.5V is 82.7mA cm -2 , 10mA cm -2 The overpotential is only 167mV at a current density of 1.57kV, and the dissolution of Ru is suppressed. It can work continuously for 300 hours in acid with stable performance. In situ experiments and theoretical calculations show that the nanoscale proximity characteristics of RuO2 / MoO3 create a rich binary interface, at which the oxygen intermediates formed on RuO2 overflow to MoO3. Therefore, the lattice oxygen of MoO3 replaces the lattice oxygen of RuO2 to participate in the formation of oxygen-oxygen intermediates, avoiding the formation of oxygen vacancies on RuO2. In turn, the excessive oxidation of ruthenium species on the surface of RuO2 can be suppressed, thereby improving the stability of oxygen evolution catalysis in acidic electrolytes.

[0022] 2. The present invention provides a new electrocatalyst for the acidic oxygen evolution reaction with high activity and high stability, and the preparation method is simple, environmentally friendly, easy to control and scalable, with strong applicability, and can be extended to the preparation and large-scale production of other electrocatalytic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] For ease of explanation, the present invention is described in detail with reference to the following specific embodiments and the accompanying drawings.

[0024] Figure 1 These are microscope images and scanning images of the RuO2 / MoO3 composite nanowire electrocatalyst prepared in Example 1. Among them, a is a transmission electron microscope image, b and c are high-angle annular dark field scanning transmission electron microscope images, d is a high-resolution transmission electron microscope image, and e is an element distribution scanning image.

[0025] Figure 2 These are the X-ray diffraction patterns and Raman patterns of the RuO2 / MoO3 composite nanowire electrocatalyst prepared in Example 1.

[0026] Figure 3 The RuO2 / MoO3 composite nanowire electrode of Example 1 was subjected to a scan rate of 10 mV s in a 0.5 M H2SO4 electrolyte. -1 The oxygen evolution polarization curves obtained under the conditions and the current density of 10 mA cm -2 Schematic diagram of the overpotential and current density at 1.5V.

[0027] Figure 4The RuO2 / MoO3 composite nanowire electrode, c-RuO2 electrode and self-made RuO2 nanowire electrode in Example 1 were -2 Schematic diagram of the chronopotentiometry test.

[0028] Figure 5 It is a schematic diagram comparing the catalytic performance of the RuO2 / MoO3 composite nanowire electrodes of Examples 1 to 3.

[0029] Figure 6 TEM images of the RuO2 / MoO3 composite nanowire electrocatalysts prepared in Examples 1, 4, and 5.

[0030] Figure 7 It is the X-ray scattering diagram of the RuO2 / MoO3 composite nanowire electrocatalyst prepared in Examples 1, 4, and 5.

[0031] Figure 8 It is a schematic diagram comparing the catalytic performance of the RuO2 / MoO3 composite nanowire electrodes of Examples 1, 4, and 5. DETAILED DESCRIPTION

[0032] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments; in the following description, specific details such as specific configurations are provided only to help fully understand the embodiments of the present invention. Therefore, it should be clear to those skilled in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present invention.

[0033] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0034] Unless otherwise specified, the materials, practices and experimental equipment involved in the implementation cases of the present invention are all in line with commercially available products in the relevant chemical and biotechnology fields.

[0035] Example 1

[0036] Step 1: Preparation of electrospinning sol

[0037] 400 mg of PVP was dissolved in 1.6 mL of DMF and mechanically stirred for 6 h to obtain a PVP solution; 70.6 mg (0.34 mmol) of RuCl3·3H2O was dissolved in 1 mL of DMF to obtain a RuCl3 solution; 10.6 mg (0.06 mmol) of (NH4)6Mo7O 24 4H2O was dissolved in 500μL deionized water to obtain (NH4)6Mo7O 24Solution; drop RuCl3 solution into PVP solution, stir for 6h, then drop (NH4)6Mo7O 24 The solution was stirred for 10 h to obtain an electrospinning sol;

[0038] Step 2: Electrospinning to prepare nanofibers

[0039] After the electrospinning sol was allowed to stand for 2 h, it was placed in a syringe and ejected from a syringe pump at a flow rate of 3 μL / min using an electrospinning system. The distance between the metal needle and the aluminum foil was fixed at 15 cm, and the external magnetic field was 13 kV. Then, the electrospun nanofibers were collected from the aluminum foil.

[0040] Step 3: Preparation of RuO2 / MoO3 composite nanowire electrocatalyst

[0041] The electrospun nanofibers were exposed to air for 1 day, and then the nanofibers were transferred to a quartz tube, heated to 350°C at a heating rate of 3°C / min in an air atmosphere, calcined at a constant temperature for 6 hours, and cooled to room temperature to obtain a RuO2 / MoO3 composite nanowire electrocatalyst.

[0042] Depend on Figure 1 (a) It can be seen that the diameter of the obtained RuO2 / MoO3 composite nanowires is about 30-50 nm, the length is 1-5 μm, and they have a uniform linear morphology. Figure 1 (b) and (c) show that RuO2 / MoO3 composite nanowires are composed of stacked nanoparticles. Figure 1 (d) It is clearly shown that RuO2 / MoO3 has lattice fringes of RuO2 and MoO3, indicating that it is a heterojunction structure. Figure 1 (e) This indicates that the elements in the RuO2 / MoO3 composite nanowires are evenly distributed, and further indicates that RuO2 and MoO3 are evenly distributed. Figure 2 It can be seen that RuO2 / MoO3 has an X-ray diffraction pattern similar to that of rutile phase RuO2, and has obvious Raman characteristic peaks of RuO2 and MoO3, which further indicates that RuO2 / MoO3 composite nanowires are formed by the accumulation of RuO2 and MoO3 nanoparticles.

[0043] Example 2

[0044] In step 1 of this example, 400 mg of PVP was dissolved in 1.6 mL of DMF and mechanically stirred for 6 h to obtain a PVP solution; 74.7 mg (0.36 mmol) of RuCl3·3H2O was dissolved in 1 mL of DMF to obtain a RuCl3 solution; 7.1 mg (0.04 mmol) of (NH4)6Mo7O 24 4H2O was dissolved in 500μL deionized water to obtain (NH4)6Mo7O24 Solution; drop RuCl3 solution into PVP solution, stir for 6h, then drop (NH4)6Mo7O 24 The solution was stirred for 10 hours to obtain an electrospinning sol. The other steps were the same as those in Example 1 to obtain an amorphous RuO2 / MoO3 composite nanowire electrocatalyst.

[0045] Example 3

[0046] In step 1 of this example, 400 mg of PVP was dissolved in 1.6 mL of DMF and mechanically stirred for 6 h to obtain a PVP solution; 66.4 mg (0.32 mmol) of RuCl3·3H2O was dissolved in 1 mL of DMF to obtain a RuCl3 solution; 14.1 mg (0.04 mmol) of (NH4)6Mo7O 24 4H2O was dissolved in 500μL deionized water to obtain (NH4)6Mo7O 24 Solution; drop RuCl3 solution into PVP solution, stir for 6h, then drop (NH4)6Mo7O 24 The solution was stirred for 10 hours to obtain an electrospinning sol. The other steps were the same as those in Example 1 to obtain a RuO2 / MoO3 composite nanowire electrocatalyst.

[0047] Example 4

[0048] In step 3 of this embodiment, the electrospun nanofibers are exposed to air for 1 day, and then the nanofibers are transferred to a quartz tube, heated to 250°C at a heating rate of 3°C / min in an air atmosphere, and calcined at a constant temperature for 6 hours. The other steps are the same as in embodiment 1 to obtain a RuO2 / MoO3 composite nanowire electrocatalyst.

[0049] Example 5

[0050] In step 3 of this embodiment, the electrospun nanofibers are exposed to air for 1 day, and then the nanofibers are transferred to a quartz tube, heated to 450°C at a heating rate of 3°C / min in an air atmosphere, and calcined at a constant temperature for 6 hours. The other steps are the same as in embodiment 1 to obtain a RuO2 / MoO3 composite nanowire electrocatalyst.

[0051] 4 mg of the RuO2 / MoO3 composite nanowire catalyst prepared in Example 1 was added with 768 μL of deionized water, 200 μL of ethanol, and 32 μL of a 5% Nafion solution. The solution was ultrasonicated for 2 h to obtain a uniform catalyst solution. Then 10 μL of the catalyst solution was taken and heated at 0.56 mg / cm 2The RuO2 / MoO3 composite nanowire electrode was prepared by loading the RuO2 / MoO3 composite nanowire electrode on carbon paper. The RuO2 / MoO3 composite nanowire electrode was tested in 0.5M H2SO4 electrolyte at a scan rate of 10mV s -1 Oxygen evolution polarization curve under the conditions. Figure 3 It can be seen that the current density of the RuO2 / MoO3 composite nanowire electrode is 82.7 mA cm at 1.5 V. -2 , 10mA cm -2 The overpotential is only 167mV at a current density of 10000mA cm. Compared with the c-RuO2 electrode and the homemade RuO2 nanowire electrode, the RuO2 / MoO3 composite nanowire electrode has excellent oxygen evolution electrocatalytic performance. At the same time, the obtained RuO2 / MoO3 composite nanowire electrode, the c-RuO2 electrode and the homemade RuO2 nanowire electrode were measured to have a good electrocatalytic performance at 10mA cm -2 The timing voltage under Figure 4 It can be seen that the presence of MoO3 greatly improves the stability of RuO2. The results show that the RuO2 / MoO3 composite nanowire electrode has a current density of 10 mA cm in 0.5 M H2SO4 electrolyte. -2 After continuous operation for 300 h under the conditions of , the attenuation of oxygen evolution performance was negligible. In contrast, the overpotential of the homemade RuO2 nanowire electrode increased by 120 mV within 150 h, while the catalytic activity of c-RuO2 decayed rapidly within 3 h.

[0052] In order to study the effect of the molar ratio of RuO2 to MoO3 in the RuO2 / MoO3 composite nanowire catalyst on the oxygen evolution catalytic performance, the RuO2 / MoO3 composite nanowire electrocatalysts prepared in Examples 1, 2, and 3 (named RuO2 / MoO3-y, where y represents the molar percentage of MoO3 in RuO2 and MoO3) were subjected to a scan rate of 10 mV s in a 0.5 M H2SO4 electrolyte. -1 The electrocatalytic performance under the conditions was tested, and the c-RuO2 electrode was compared with the homemade RuO2 nanowires. Figure 5 It can be seen that when the molar ratio of RuO2 to MoO3 is 8.5:1.5, the oxygen evolution catalytic performance is optimal.

[0053] In order to study the effect of calcination temperature on the morphology, crystal structure and oxygen evolution catalytic performance of RuO2 / MoO3 composite nanowire catalysts, the RuO2 / MoO3 composite nanowire electrocatalysts prepared at different calcination temperatures in the above Examples 1, 4 and 5 were characterized in morphology and compared in catalytic performance (named RuO2 / MoO3-0.15-z, where z represents the calcination temperature). Figure 6 The morphologies of the corresponding catalysts at different calcination temperatures are shown, and the catalysts all present nanowire morphology. Figure 7 The XRD patterns of the corresponding catalysts at calcination temperatures of 250°C, 350°C, and 450°C show that when the calcination temperature is 350°C and 450°C, the catalyst presents a rutile phase structure. Figure 8 The results show that the corresponding catalysts were calcined at 250°C, 350°C, and 400°C in 0.5 M H2SO4 at a scan rate of 10 mV s -1 From the oxygen evolution polarization curve, it can be seen that the RuO2 / MoO3 composite nanowire electrode prepared at a calcination temperature of 350°C has better acidic oxygen evolution catalytic performance.

[0054] Those skilled in the art to which the present application belongs may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but they will not deviate from the inventive concept of the present application or exceed the scope defined by the attached claims.

Claims

1. A RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction, characterized in that: The electrocatalyst is a nanowire formed by stacking RuO2 and MoO3 nanoparticles, the diameter of the nanowire is 30-50nm, the length is 1-5μm, and the molar ratio of RuO2 to MoO3 is 9:1-8:

2.

2. The RuO2 / MoO3 composite nanowire electrocatalyst for acidic oxygen evolution reaction according to claim 1, characterized in that: In the electrocatalyst, the molar ratio of RuO2 to MoO3 is 8.5:1.

5.

3. A method for preparing the electrocatalyst according to claim 1 or 2, characterized in that: The specific steps include: Step 1: Preparation of electrospinning sol: Dissolving polyvinyl pyrrolidone and ruthenium trichloride in N,N-dimethylformamide respectively, dissolving ammonium molybdate in deionized water, then dropping the ruthenium trichloride solution into the polyvinyl pyrrolidone solution, stirring for 4 to 8 hours, then dropping the ammonium molybdate solution, stirring for 8 to 12 hours, to obtain an electrospinning sol; Step 2: Electrospinning to prepare nanofibers: After the electrospinning sol was allowed to stand for 1 to 2 hours, it was placed in a syringe and electrospun into nanofibers using an electrospinning system; Step 3: Preparation of RuO2 / MoO3 composite nanowire electrocatalyst: The nanofibers are exposed to air for 20 to 24 hours, then transferred to a quartz tube, calcined at 200 to 500° C. for 4 to 8 hours in an air atmosphere, and cooled to room temperature to obtain a RuO2 / MoO3 composite nanowire electrocatalyst.

4. The method for preparing an electrocatalyst according to claim 3, characterized in that: In step 1, the concentration of polyvinyl pyrrolidone in the electrospinning sol is 100-200 mg / mL, the concentration of ruthenium trichloride is 10-30 mg / mL, the concentration of ammonium molybdate is 1-10 mg / mL, and the volume ratio of N,N-dimethylformamide to deionized water is 2:1-6:

1.

5. The method for preparing an electrocatalyst according to claim 3, characterized in that: In step 1, the concentration of polyvinyl pyrrolidone in the electrospinning sol is 130-150 mg / mL, the concentration of ruthenium trichloride is 20-25 mg / mL, the concentration of ammonium molybdate is 2-4 mg / mL, and the volume ratio of N,N-dimethylformamide to deionized water is 4:1-5:

1.

6. The method for preparing an electrocatalyst according to claim 3, characterized in that: In step 2, the electrospinning sol is ejected from a syringe pump at a flow rate of 1 to 10 μL / min using an electrospinning system, the distance between the metal needle and the aluminum foil is fixed at 15 to 20 cm, and the external magnetic field is 10 to 14 kV.

7. The method for preparing an electrocatalyst according to claim 3, characterized in that: In step 3, calcination is performed at 350° C. in an air atmosphere for 5 to 8 hours.

8. The method for preparing an electrocatalyst according to claim 3, characterized in that: In step 3, the heating rate of the calcination is 2 to 5°C / min.

Citation Information

Cited By

  • Transition metal anchored heteroatom doped RuO2 fiber aerogel electrocatalyst as well as preparation method and application thereof

    CN120905702A