Glass-based packaging carrier plate electroplating hole-filling leveling agent, electroplating liquid and electroplating hole-filling method

By using alternating copolymers of tetrachloromethylmethane and tertiary amine-containing structural ethers as leveling agents, combined with segmented electroplating technology, the thickness uniformity and deep plating capacity in glass through-hole electroplating fillers is solved, and high efficiency is achieved plating control and cost reduction.

CN118910686APending Publication Date: 2024-11-08KUN SHAN FRJ TECH LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411172030.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing glass through-hole technology has problems with thickness uniformity during the electroplating and filling process, poor deep plating capacity, large additive consumption, and cannot be effectively applied to high aspect ratio glass through-hole filling.

Method used

A polyquaternary ammonium salt is used as the electroplating hole-filling leveling agent. The leveling agent is an alternating copolymer of tetrachloromethylmethane and ethers containing tertiary amine structure. It has a high branching structure and good water solubility, and can control pores. The inner copper plating speed and surface copper thickness are optimized, and the current density and time are optimized through the segmented electroplating method to improve the dispersion and coverage capacity of the plating solution.

Benefits of technology

While filling the hole, the copper thickness on the control surface is within a thin range, ensuring uniformity and density of the coating. It is suitable for high aspect ratio glass through-hole filling, reducing production costs and additive consumption, and improving quality and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910686A_ABST
    Figure CN118910686A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electroplating with glass as a packaging carrier plate, and particularly relates to a glass-based packaging carrier plate electroplating hole-filling leveling agent, electroplating liquid and an electroplating hole-filling method. The leveling agent for electroplating and hole filling of the glass-based packaging substrate is polyquaternary ammonium salt, and the polyquaternary ammonium salt is an alternating copolymer of tetrachloromethylmethane and ether containing a tertiary amine structure. According to the method, the surface copper can be controlled to be thin while the holes are filled, the hole filling performance is excellent, subsequent fine circuit manufacturing is facilitated, and the surface copper can be more uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention belongs to the field of electroplating technology of glass as packaging substrate, and specifically relates to electroplating hole filling leveling agent, electroplating solution and electroplating hole filling method for glass-based packaging substrate. Background Art

[0002] Through Silicon Via (TSV) technology is a high-density packaging technology that achieves vertical electrical interconnection of silicon vias by filling conductive materials such as copper, tungsten, and polysilicon. At present, through silicon via technology (TSV) is relatively mature and has been widely used in actual production, but silicon is a semiconductor material. Under the action of electric or magnetic fields, the carriers around it can move freely, which may interfere with adjacent circuits or signals, thereby affecting the performance of the chip. Therefore, the cost of silicon-based adapters is high and the electrical performance is poor, which limits their market application.

[0003] Glass materials have excellent dielectric properties, a thermal expansion coefficient close to that of silicon, and good mechanical stability. Even at very thin thicknesses, warping is very small. In addition, large-size glass panels are easy to obtain, which reduces process complexity and processing costs, and does not require the production of insulating layers. Therefore, through-glass vias (TGVs) and related technologies have broad application prospects in optical communications, radio frequency, microwaves, microelectromechanical systems, microfluidic devices, and three-dimensional integration. They are expected to replace TSVs in some scenarios and become one of the core evolution directions of advanced packaging in the AI ​​era. Intel has hailed them as "new game changers."

[0004] Up to now, the high-quality filling technology of TGV is one of the main difficulties in the development of glass through-hole three-dimensional interconnection technology. Since it is difficult for the current to be uniform across the entire glass substrate, there is a problem of thickness uniformity in the TGV electroplating process. In addition, the high-quality filling technology of TGV is different from that of TSV. The aperture of TGV is relatively large and most of them are through holes. In the electroplating filling process of the existing technology, as the copper ions in the hole are deposited, the thickness of the surface copper plating layer has been increasing. For the subsequent fine circuit production, the surface copper thickness needs to be reduced to below the required thickness of the circuit. The existing hole filling copper plating is sulfate copper plating, which is mainly based on sulfuric acid, copper sulfate, and chloride ions. It is achieved by adding accelerators, inhibitors, and leveling agents. The leveling agent is usually a nitrogen-containing heterocyclic compound. Its deep plating ability and dispersion ability can only meet the relatively low-end TSV hole filling. High-end TSV technology is subject to others in terms of equipment, raw materials, and processes. In addition, the existing leveling agent also needs to cooperate with accelerators and inhibitors to cooperate with each other. Only when the three additives reach a suitable ratio can a better filling effect be obtained when filling TSV holes. In summary, existing electroplating solutions and levelers have problems such as complex ingredients, low hole filling efficiency, poor deep plating ability, large additive consumption, and thick copper plated surface, and are not well suited for TGV, especially high aspect ratio TGV through-hole filling. Summary of the invention

[0005] One of the purposes of the present invention is to provide a glass-based packaging substrate electroplating hole filling leveling agent, which is beneficial for filling the holes while controlling the surface copper to a thinner thickness, has excellent hole filling performance, is beneficial for subsequent fine circuit production, and can make the surface copper more uniform.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A glass-based packaging substrate electroplating hole filling leveler, the leveler is a polyquaternary ammonium salt, the polyquaternary ammonium salt is an alternating copolymer of tetrachloromethylmethane and an ether containing a tertiary amine structure, and the structural formula of the ether containing a tertiary amine structure is:

[0008]

[0009] Wherein, R1, R2, R3, and R4 can each independently be a methyl group or an ethyl group, and R5 and R6 can each independently be a C1-C6 straight-chain alkylene group or a branched alkylene group.

[0010] The polyquaternary ammonium salt of the present invention is an alternating copolymer of ether containing a tertiary amine structure and tetrachloromethylmethane, which contains a highly branched dendritic structure and has good water solubility. Moreover, since the macromolecular polymer is relatively difficult to enter the pores, the number of complexed copper ions in the pores is relatively small, thereby increasing the copper plating speed in the pores, thus being conducive to the growth of the pore copper and the control of the surface copper thickness, and having a good deep plating effect. In addition, the leveling agent of the polyquaternary ammonium salt of the present invention can improve the dispersibility and covering ability of the plating solution. Since the amine-containing functional group carries a positive charge, it is easy to be adsorbed in high current density areas, especially in areas where the plate surface is protruding (where the copper thickness is thicker), so the copper deposition in these parts can be reduced, making the coating surface more uniform and also conducive to making the coating more compact.

[0011] Furthermore, the ether containing a tertiary amine structure may be a symmetrical amine ether or an asymmetrical amine ether, preferably a symmetrical amine ether because the raw materials are easier to obtain.

[0012] Furthermore, the ether containing a tertiary amine structure is preferably di[2-(N,N-dimethylaminoethyl)]ether, or di[3-(N,N-dimethylaminopropyl)]ether or dimethylaminoethyl dimethylaminopropyl ether.

[0013] Furthermore, the molecular weight of the polyquaternary ammonium salt leveler is 3000 to 8000. The invention can facilitate the growth of pore copper and control of surface copper thickness by adding a polyquaternary ammonium salt compound with a molecular weight greater than 3000 and less than 8000 into the electrolytic solution, and has a good deep plating effect.

[0014] The leveling agent based on the polyquaternary ammonium salt of the present invention has the advantages of good water solubility and strong adaptability, and can be used together with an inhibitor and an accelerator, or can be used only with an accelerator.

[0015] The leveling agent based on the polyquaternary ammonium salt of the present invention can be used alone as a leveling agent, or can be used together with other leveling agent compounds as a leveling agent.

[0016] The preparation method of the above-mentioned glass-based packaging substrate electroplating hole filling leveling agent is as follows: tetrachloromethylmethane and ether containing a tertiary amine structure are added to a solvent, mixed, heated, and the above-mentioned polyquaternary ammonium salt leveling agent is obtained after the reaction is completed. The solvent can be methanol, ethanol, propanol or ethylene glycol.

[0017] Furthermore, the molar ratio of tetrachloromethylmethane to the ether containing a tertiary amine structure is 1: (1-3), the heating temperature is 50-130° C., and the reaction is carried out for more than 5 hours. In addition, by controlling the polymerization reaction time and the ratio of the reaction raw materials, the molecular weight of the leveling agent can be controlled to a certain extent so that the molecular weight is within the desired range, and at the same time, it can also ensure that the polymerization reaction is fully and thoroughly carried out.

[0018] The invention also relates to the application of the leveling agent in electroplating and hole filling of a glass-based packaging carrier.

[0019] Furthermore, when the leveling agent is used for electroplating hole filling, the hole filled by electroplating can be one or more of a through hole, a blind hole, and a buried hole.

[0020] The present invention also discloses an electroplating solution containing the above-mentioned leveling agent. In some possible implementations, when the leveling agent is applied to electroplating hole filling, the electroplating solution used includes a solution containing copper ions, an inorganic additive, and an organic additive. In the electroplating solution, the inorganic additive includes a ferrous chloride solution. Adding a ferrous chloride solution can be beneficial to the growth of hole copper, and the deep plating effect is good, wherein the chloride ions can synergistically act with the electroplating additives, and the ferrous ions can help stabilize the additives, reduce the consumption of the additives, and reduce the deposition rate of the surface copper, thereby reducing the thickness of the surface copper. The organic solvent includes an accelerator, or includes an accelerator and an inhibitor.

[0021] Furthermore, in the electroplating solution, the amount of the leveling agent based on the polyquaternary ammonium salt can be 20 to 350 mg / L, wherein the best effect is achieved when the amount is 50 to 150 mg / L. The consumption of the leveling agent in the electroplating process of the present invention is small, and the consumed product does not cause the liquid to be denatured, so the electroplating tank does not need to be updated for a long time, which helps to reduce costs and improve quality.

[0022] In some possible implementations, the present invention further provides an electroplating method using an electroplating solution containing the above-mentioned leveling agent, wherein the electroplating hole filling operation is as follows: segmented electroplating is adopted, and the electroplating current is direct current, wherein starting from the third segment, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package carrier, as follows:

[0023] The first stage: forward current electroplating, current density is 1ASf, time is 10~15min;

[0024] The second stage: forward current electroplating, current density is 2ASf, time is 30~60min;

[0025] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 5-120min;

[0026] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 60 to 180min;

[0027] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:2) to (2:1), and the total electroplating time of the fifth stage current is 10 to 120min;

[0028] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:3), and the total electroplating time of the sixth stage current is 60 to 120min;

[0029] The seventh stage: the current density is 3-5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20-30ms, the forward and reverse pulse time ratio is (1:1)-(1:3), and the total electroplating time of the seventh stage current is greater than or equal to 0min and less than or equal to 60min.

[0030] Specifically, compared with the existing technology, this technology can produce the following positive effects:

[0031] 1. The leveling agent of the polyquaternary ammonium salt of the present invention has excellent hole filling performance. It can ensure that the hole is filled while the surface copper can be controlled at a thinner thickness, which is beneficial to the subsequent fine circuit production, and the surface copper can be made more uniform. It can be applicable to TGV, even for TGV through holes with high aspect ratio, and can also play a good hole filling performance, and can significantly reduce the surface copper layer thickness and the hole center copper layer thickness ratio. In addition, the leveling agent of the polyquaternary ammonium salt of the present invention is easy to synthesize, and the raw material is easily obtained, and the synthetic route is short and the reaction is simple. Therefore, it has a good and wide market application prospect.

[0032] 2. The consumption of leveling agent in the electroplating process of the present invention is small, and the consumed product will not cause the syrup to denature, so the electroplating tank does not need to be updated for a long time, which helps to reduce costs and improve quality.

[0033] 3. The leveling agent of the polyquaternary ammonium salt of the present invention is combined with the method of segmented electroplating hole filling, which can further improve the distribution of hole copper and surface copper thickness. By reasonably designing the forward and reverse current density and time, the thickness of the hole copper can be guaranteed, the hole is filled solid, and it is not easy to fall off, and the surface copper can be further controlled to a thinner thickness, which is beneficial to the subsequent fine circuit production. At the same time, since the present invention does not need a subsequent copper reduction process, the production cost is reduced, and the copper surface uniformity and flatness are better, so the present invention has a high yield rate, more reliable quality, and simpler process. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a hole filling effect diagram of Example 10 of the present invention;

[0035] Figure 2 This is a hole filling effect diagram of Example 11 of the present invention;

[0036] Figure 3 This is a hole filling effect diagram (one) of Example 12 of the present invention;

[0037] Figure 4 This is the hole filling effect diagram (part 2) of Example 12 of the present invention. DETAILED DESCRIPTION

[0038] The following examples are provided to facilitate a better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified.

[0039] Example 1

[0040] This embodiment provides a method for preparing a polyquaternary ammonium salt leveler polytetrachloromethylmethane-bis[2-(N,N-dimethylaminoethyl)]ether quaternary ammonium salt:

[0041] Weigh 21g (i.e. 0.1mol) of tetrachloromethylmethane, 32g (i.e. 0.2mol) of di[2-(N,N-dimethylaminoethyl)]ether and 180ml of anhydrous ethanol respectively, pour the weighed tetrachloromethylmethane, di[2-(N,N-dimethylaminoethyl)]ether and anhydrous ethanol into a reaction container, stir evenly at room temperature, and heat to 60°C under the protection of an inert gas (such as nitrogen). Keep the constant temperature reaction for 18h, cool, remove the ethanol under reduced pressure, and obtain a polyquaternary ammonium salt leveler after recrystallization: polytetrachloromethylmethane-di[2-(N,N-dimethylaminoethyl)]ether quaternary ammonium salt.

[0042] Example 2

[0043] This embodiment provides another method for preparing a polyquaternary ammonium salt leveler polytetrachloromethylmethane-bis[3-(N,N-dimethylaminopropyl)]ether quaternary ammonium salt

[0044] Weigh 21 g (i.e. 0.1 mol) of tetrachloromethylmethane, 37.6 g (i.e. 0.2 mol) of di[3-(N,N-dimethylaminopropyl)]ether and 180 ml of anhydrous ethanol respectively, pour the weighed tetrachloromethylmethane, di[3-(N,N-dimethylaminopropyl)]ether and anhydrous ethanol into a reaction container, stir evenly at room temperature, and heat to 90°C under the protection of an inert gas (such as nitrogen). Keep the constant temperature reaction for 14 hours, cool, remove the ethanol under reduced pressure, and obtain a polyquaternary ammonium salt leveler after recrystallization: polytetrachloromethylmethane-di[3-(N,N-dimethylaminopropyl)]ether quaternary ammonium salt.

[0045] Example 3

[0046] This embodiment provides another method for preparing a polyquaternary ammonium salt leveler, polytetrachloromethylmethane-dimethylaminoethyldimethylaminopropyl ether quaternary ammonium salt:

[0047] Weigh 21 g (i.e. 0.1 mol) of tetrachloromethylmethane, 34.8 g (i.e. 0.2 mol) of dimethylaminoethyl dimethylaminopropyl ether and 180 ml of anhydrous ethanol respectively, pour the weighed tetrachloromethylmethane, dimethylaminoethyl dimethylaminopropyl ether and anhydrous ethanol into a reaction container, stir evenly at room temperature, and heat to 80°C under the protection of an inert gas (such as nitrogen). Keep the constant temperature reaction for 15 hours, cool, remove the ethanol under reduced pressure, and obtain a polyquaternary ammonium salt leveler after recrystallization: polytetrachloromethylmethane-dimethylaminoethyl dimethylaminopropyl ether quaternary ammonium salt.

[0048] The electroplating solution of the present invention can be prepared according to the following component contents: 100-240 g / L of copper sulfate pentahydrate, 30-60 g / L of sulfuric acid (98%), 80-180 mg / L of ferrous chloride, and a leveler, and may also include an accelerator, or include an accelerator and an inhibitor. Among them, the leveler can be the polyquaternary ammonium salt leveler of the present invention alone, or it can be the polyquaternary ammonium salt leveler of the present invention in combination with other leveler compounds. The above-mentioned accelerator is generally a sulfur-containing compound, such as a compound containing a disulfide bond and its salt, a compound containing a sulfonic acid group and its salt, a thiol, a phosphate, etc., such as SPS, MPS, etc. The inhibitor is generally a polymer containing an oxygen bonding structure, such as PEG (polyethylene glycol), PPG (polypropylene glycol), etc. Chloride ions can produce a synergistic inhibition or synergistic acceleration effect on copper deposition with other additives.

[0049] Example 4

[0050] The present embodiment provides an electroplating solution, which includes 50 mg / L of the polyquaternary ammonium salt synthesized in Example 1 (as a leveling agent); and also includes 220 g / L of copper sulfate pentahydrate, 60 g / L of sulfuric acid (98%), 85 mg / L of ferrous chloride, 20 mg / L of sodium polydisulfide propane sulfonate (SPS), and 300 mg / L of PEG (polyethylene glycol).

[0051] The above-mentioned electroplating solution is used to electroplate and fill holes in the TGV to be plated. The glass substrate to be plated (i.e., glass-based packaging carrier, sometimes referred to as substrate) has a thickness of 388.2 μm, a minimum hole diameter of 92.6 μm, and an aspect ratio of about 4.2:1. Before electroplating, the substrate to be plated is pre-metallized on the plate surface and in the hole; the electroplating current density is 1.5 A / dm 2 , the electroplating temperature is 25℃, air stirring, and the electroplating time is 90min.

[0052] Example 5

[0053] The present embodiment is different from the embodiment 4 in that the polyquaternium salt 50 mg / L in the embodiment 4 is replaced by 100 mg / L.

[0054] Example 6

[0055] The present embodiment is different from the embodiment 4 in that the polyquaternium salt 50 mg / L in the embodiment 4 is replaced by 200 mg / L.

[0056] Example 7

[0057] The difference between this embodiment and embodiment 4 is that the leveling agent used in embodiment 4 is replaced by the polyquaternary ammonium salt synthesized in embodiment 2 (as the leveling agent), and the dosage is 50 mg / L.

[0058] Example 8

[0059] The present embodiment is different from the embodiment 7 in that 50 mg / L of the polyquaternary ammonium salt (i.e., the polyquaternary ammonium salt synthesized in the embodiment 2) in the embodiment 7 is replaced by 100 mg / L.

[0060] Example 9

[0061] The present embodiment is different from the embodiment 7 in that 50 mg / L of the polyquaternary ammonium salt (i.e., the polyquaternary ammonium salt synthesized in the embodiment 2) in the embodiment 7 is replaced by 200 mg / L.

[0062] The results show that the polyquaternary ammonium salt leveling agent of Examples 4 to 9 of the present invention has excellent hole filling performance. When the holes are filled, Examples 4 to 9 of the present invention can control the surface copper thickness within 7.8-12.1 μm, and the surface copper is uniform, the surface is bright, and has better flatness.

[0063] The feasibility of using the polyquaternary ammonium salt of the present invention as an electroplating hole filling and leveling agent is further verified by the following comparative examples:

[0064] Example 10

[0065] The present embodiment provides an electroplating solution, which includes 100 mg / L of the polyquaternary ammonium salt synthesized in Example 1 (as a leveling agent), 220 g / L of copper sulfate pentahydrate, 60 g / L of sulfuric acid (98%), 85 mg / L of ferrous chloride, 20 mg / L of sodium polydisulfide propane sulfonate (SPS), and 300 mg / L of PEG (polyethylene glycol).

[0066] The above-mentioned electroplating solution is used to electroplate and fill holes in the TGV to be plated. The glass substrate to be plated has a thickness of 388.2 μm, a minimum pore size of 92.6 μm, and an aspect ratio of about 4.2:1. Before electroplating, the substrate to be plated is pre-metallized on the board surface and in the hole; the process of electroplating and filling holes is as follows: segmented electroplating is used, and the electroplating process includes six segments of electroplating, from the first segment to the sixth segment, the electroplating current is direct current, and the forward and reverse pulse currents are alternately switched from the third segment to reduce the thickness of the surface copper electroplated on the surface of the glass-based package carrier, as follows:

[0067] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0068] The second stage: forward current electroplating, current density is 2ASf, time is 45min;

[0069] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100ms, the forward and reverse pulse time ratio is 2:1, and the total electroplating time of the third stage current is 35min;

[0070] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time can be 100ms, the forward and reverse pulse time ratio is 2:1, and the total electroplating time of the fourth stage current is 70min;

[0071] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the fifth stage current is 20min;

[0072] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30ms, the forward and reverse pulse time ratio is 1:1.5, and the total electroplating time of the sixth stage current is 65min.

[0073] Electroplating hole filling effect Figure 1 shown.

[0074] Embodiment 11

[0075] The present embodiment provides an electroplating solution, which includes 100 mg / L of the polyquaternary ammonium salt synthesized in Example 1 (as a leveling agent); and also includes 220 g / L of copper sulfate pentahydrate, 60 g / L of sulfuric acid (98%), 85 mg / L of ferrous chloride, 20 mg / L of sodium polydisulfide propane sulfonate (SPS), and 300 mg / L of PEG (polyethylene glycol).

[0076] The above-mentioned electroplating solution is used to electroplate and fill holes in the TGV to be plated. The glass substrate to be plated has a thickness of about 425 μm, a minimum hole diameter of about 70 μm, and an aspect ratio of about 6:1. Before electroplating, the substrate to be plated is pre-metallized on the plate surface and in the hole; the electroplating current density is 1.5 A / dm 2 , the electroplating temperature is 25℃, air stirring, and the electroplating time is 90min.

[0077] Electroplating hole filling effect Figure 2 shown.

[0078] Example 12

[0079] This example is a comparative example. The plating solution used in this example is a commonly used plating solution formula in the prior art, and its components are as follows: the leveling agent is denazur green, the dosage is 6 mg / L; copper sulfate pentahydrate 220 g / L, sulfuric acid (98%) 60 g / L, chloride ion 36 mg / L, sodium polydisulfide bispropane sulfonate (SPS) 6 mg / L, PEG (polyethylene glycol) 600 mg / L.

[0080] The above-mentioned electroplating solution is used to electroplate and fill holes in the TGV to be plated. The glass substrate to be plated has a thickness of about 425 μm, a minimum hole diameter of about 70 μm, and an aspect ratio of about 6:1. Before electroplating, the substrate to be plated is pre-metallized on the plate surface and in the hole; the electroplating current density is 1.5 A / dm 2 , the electroplating temperature is 25℃, air stirring, and the electroplating time is 90min.

[0081] Electroplating hole filling effect Figure 3-Figure 4 As shown, the experimental results show that the plated parts of this embodiment (i.e., embodiment 12) have significantly higher hole cracks than embodiments 4 to 11 of the present invention, and the surface copper thickness is also significantly higher than that of the present invention. The polyquaternary ammonium salt of the present invention is an alternating copolymer of an ether containing a tertiary amine structure and tetrachloromethylmethane, which contains a highly branched dendritic structure and has good water solubility. Moreover, since the macromolecular polymer is relatively difficult to enter the pores, the number of complexed copper ions in the pores is relatively small, thereby increasing the copper plating speed in the pores, which is beneficial to the growth of the pore copper and the control of the surface copper thickness, and has a good deep plating effect. In addition, the leveling agent of the polyquaternary ammonium salt of the present invention can improve the dispersibility and covering ability of the plating solution. Since the amine-containing functional group carries a positive charge, it is easy to adsorb on high current density areas, especially on protruding areas on the board surface (where the copper thickness is thicker), so it can reduce copper deposition in these areas, making the coating surface more uniform, and also conducive to making the coating denser. For reference, Figure 1 , Figure 2 In addition, since the polyquaternary ammonium salt leveling agent of the present invention has the advantages of good water solubility and strong adaptability, it has a wide range of application prospects.

[0082] In addition, Examples 4 to 11 are merely examples of the present invention. The leveling agent based on the above-mentioned polyquaternary ammonium salt of the present invention can be used alone as a leveling agent, or can be used together with other leveling agent compounds as a leveling agent.

[0083] As can be seen from Example 1 to Example 3, the leveling agent of the polyquaternary ammonium salt of the present invention is easy to synthesize, the raw materials are easy to obtain, the synthesis route is short, and the reaction is simple. As can be seen from Example 4 to Example 11, the leveling agent of the polyquaternary ammonium salt of the present invention has excellent hole filling performance, can ensure that the hole is filled, and can also control the surface copper to a thinner thickness, which is beneficial to the subsequent fine circuit production, and can make the surface copper more uniform, can be applicable to TGV, and even for TGV through holes with high aspect ratios, can also play a good hole filling performance, can significantly reduce the surface copper layer thickness and the hole center copper layer thickness ratio. Therefore, it has a good and wide market application prospect. In addition, the leveling agent consumption in the electroplating process of the present invention is small, and the consumption product will not cause the liquid medicine to be denatured, so the electroplating tank can be updated without renewal in a long time, which helps to reduce costs and improve quality.

[0084] By comparing Example 10, Example 11, and Example 12, it can be seen that the leveling agent of the polyquaternary ammonium salt of the present invention is combined with the method of segmented electroplating hole filling, which can further improve the distribution of hole copper and surface copper thickness. The present invention can ensure the thickness of hole copper, fill the hole solid, and not fall off easily by reasonably designing the forward and reverse current density and time, and can further control the surface copper to a thinner thickness, which is beneficial to the subsequent fine circuit production. At the same time, since the present invention does not need a subsequent copper reduction process, the production cost is reduced, and the uniformity and flatness of the copper surface are better, so the present invention has a high yield rate, more reliable quality, and simpler process.

[0085] The above description is only an example of the present invention and is not intended to limit the present invention in other forms. Any technician familiar with the profession may use the technical contents disclosed above to change or modify them into equivalent embodiments with equivalent changes and apply them to other fields. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the technical solution content of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A glass-based package substrate electroplating hole filling and leveling agent, characterized in that: The leveling agent is a polyquaternary ammonium salt, which is an alternating copolymer of tetrachloromethylmethane and an ether containing a tertiary amine structure. The structural formula of the ether containing a tertiary amine structure is: Wherein, R1, R2, R3, and R4 are each independently a methyl group or an ethyl group, and R5 and R6 are each independently a C1-C6 straight-chain alkylene group or a branched alkylene group.

2. The glass-based package substrate electroplating hole filling and leveling agent according to claim 1, characterized in that: The ether containing a tertiary amine structure is di[2-(N,N-dimethylaminoethyl)]ether, or di[3-(N,N-dimethylaminopropyl)]ether or dimethylaminoethyl dimethylaminopropyl ether.

3. The glass-based package substrate electroplating hole filling and leveling agent according to claim 1, characterized in that: The molecular weight of the leveling agent is 3000-8000.

4. A method for preparing the leveling agent according to any one of claims 1 to 3, characterized in that The steps are as follows: adding tetrachloromethylmethane and ether containing a tertiary amine structure into a solvent, mixing, heating, and after the reaction is completed, the polyquaternary ammonium salt leveler is obtained, and the solvent is methanol, ethanol, propanol or ethylene glycol.

5. An electroplating solution, characterized in that: The electroplating solution comprises the leveler according to any one of claims 1 to 3.

6. The electroplating solution according to claim 5, characterized in that The dosage of leveling agent is 20-350 mg / L.

7. The electroplating solution according to claim 5, characterized in that The electroplating solution also includes a solution containing copper ions, an inorganic additive, and an organic additive. The organic additive includes an accelerator, and the inorganic additive includes a ferrous chloride solution.

8. The electroplating solution according to claim 7, characterized in that The organic additives also include inhibitors.

9. An electroplating hole filling method, characterized in that: The electroplating hole filling method comprises: using the electroplating solution of claim 5 to perform electroplating hole filling.

10. The electroplating hole filling method according to claim 9, characterized in that: The operation of electroplating hole filling is as follows: segmented electroplating is adopted, and the electroplating current is direct current. From the third segment, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package substrate, as follows: The first stage: forward current electroplating, current density is 1ASf, time is 10~15min; The second stage: forward current electroplating, current density is 2ASf, time is 30~60min; The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 5-120min; The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 60 to 180min; The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:2) to (2:1), and the total electroplating time of the fifth stage current is 10 to 120min; The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:3), and the total electroplating time of the sixth stage current is 60 to 120min; The seventh stage: the current density is 3-5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20-30ms, the forward and reverse pulse time ratio is (1:1)-(1:3), and the total electroplating time of the seventh stage current is greater than or equal to 0min and less than or equal to 60min.

Citation Information

Cited By

  • Glass adapter plate, filling method of glass through hole of glass adapter plate and chip

    CN119640351A