Green preparation method and high-valued application of pittosporum tobira fiber

Through the degumming treatment and mechanical degradation technology of choline chloride-based eutectic solvents, the high energy consumption and pollution problems of Qingtong sterilized fiber degumming process are solved, and efficient and environmentally friendly cellulose micro-nanofiber aerogel is prepared, suitable for High-value application of functional materials.

CN118910741APending Publication Date: 2024-11-08GUIZHOU JINTONG ECOLOGICAL AGRICULTURE TECHNOLOGY CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411054025.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing degumming treatment process of Qingtong bast fiber has problems such as long process, high energy consumption, and environmental pollution, and lacks new degumming methods with green, efficient and short processes.

Method used

Choline chloride-based eutectic solvent (DES) is used to deguel the phloem of Qingtong. The colloidal components are decomposed through hydrogen bond competition and proton catalytic decomposition, and the colloidal components on the surface of the fiber are removed, and cellulose micro-nanofibers are prepared in combination with mechanical degradation. and aerogel.

Benefits of technology

The preparation of Qingtong fiber with short process, high efficiency and energy saving, high fiber production rate and pollution-free is achieved. The prepared cellulose micro-nanofiber aerogel has biodegradable, recyclable and excellent mechanical elasticity, suitable for thermal insulation and environmental restoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910741A_ABST
    Figure CN118910741A_ABST
Patent Text Reader

Abstract

The invention relates to an environment-friendly preparation method and high-valued application of a pittosporum indicum fiber, and belongs to the technical field of pittosporum indicum fibers.The pittosporum indicum bast is degummed through a choline chloride deep eutectic solvent (DES), colloid components on the surface of the pittosporum indicum fiber can be effectively removed, and the method has the advantages of being short in process, efficient, capable of saving energy, high in fiber yield and the like. The choline chloride DES belongs to a green solvent, has the advantages of low cost, easiness in preparation and recyclability, is non-toxic, harmless and biodegradable, and has no pollution and zero emission in the DES one-step degumming process compared with strong acid, strong alkali and the like in traditional chemical degumming. The tung fibers subjected to DES degumming treatment are mechanically degraded into cellulose micro-nanofibers (CMNF) through simple mechanical treatment, functional materials such as CMNF aerogel are prepared through processes such as freeze drying, and high-valued application of the functional materials is achieved. Compared with traditional regenerated cellulose gel, the regenerated cellulose gel shows excellent mechanical elasticity, and has a wide application prospect in thermal insulation and environmental restoration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of Paulownia fiber, and in particular to a green preparation method of Paulownia fiber and high-value application thereof. Background Art

[0002] At present, synthetic fibers represented by polyester, polyamide and polyurethane fibers have the advantages of excellent mechanical properties, high yield, good stability and wear resistance, and have been widely used in functional textiles, composite materials, medical health and other fields. However, these synthetic fibers require complex manufacturing processes with high energy consumption and high costs. In addition, this type of fiber material is not biodegradable and difficult to recycle at the end of the product life cycle, and is not sustainable. Therefore, it is of great significance to vigorously promote the research and development of natural fiber materials as a green structural composite material.

[0003] The Chinese Paulownia belongs to the family Sterculiae and the genus Sterculia. It is popularly known as "nine-layer bark". It is a perennial deciduous tree that is easy to reproduce, has strong adaptability, grows fast, and matures in five years. Many wild Chinese Paulownia trees are found in Jianhe County, Qiandongnan Prefecture. The resources are abundant, but the utilization rate is low. The bast bark of the Chinese Paulownia can be obtained by cutting down the branches and mechanically peeling them. The main component of the bast bark of the Chinese Paulownia is cellulose fiber, which has the advantages of high mechanical strength and non-rottenness. It has long been used as a natural rope binding item. At present, the research on Chinese Paulownia mainly focuses on sowing and seedling raising and component analysis, but there are few reports on the green manufacturing and high-value application of its bast fiber. Therefore, the preparation of Chinese Paulownia tough fiber by green methods will not only broaden the source of textile fibers, but also can be processed into environmentally friendly functional materials with high industrial value, which is in line with the sustainable development strategy.

[0004] According to literature reports, in addition to cellulose, the bast of Paulownia chinensis contains colloidal components such as hemicellulose, lignin, pectin, lipid wax, water-soluble matter and ash. Therefore, the degumming treatment of Paulownia chinensis bast is crucial for the manufacture of its fiber and subsequent processing and application. In 2013, the research group first reported the degumming treatment of Paulownia chinensis bast by chemical methods using acid, alkali and other additives (Li Changlong, Liu Qiong, Sun Ruixia, Wang Zongqian*. Chemical degumming of Paulownia chinensis bast and fiber performance analysis [J]. Journal of Textile Research, 2013, 34(12): 8-11.), but it has problems such as long process, high energy consumption and environmental pollution. Therefore, it is urgent to explore and develop a new green, efficient and short-process degumming process. Deep eutectic solvent (DES) is a rapidly emerging new green solvent that can replace traditional organic solvents and ionic liquids. It was first proposed by Abbott in 2003. DES is usually a two-component or multi-component solvent system composed of a certain molar ratio of hydrogen bond acceptors and hydrogen bond donors. It has unique physical and chemical properties such as low melting point, low cost, biodegradability, designable structure, good solubility, as well as advantages such as low toxicity and recyclability. Based on the above characteristics, DES has broad application prospects in the field of biomass fiber pretreatment and conversion. However, there has been no report on the use of DES to degumming Paulownia bast, manufacturing Paulownia bast fiber and its high-value utilization in the field of functional materials.

[0005] Those skilled in the art are in urgent need of developing a green preparation method for Paulownia fiber and its high-value application to meet existing application needs and performance requirements. Summary of the invention

[0006] In view of the problems existing in the above-mentioned prior art, the present invention aims to provide a green preparation method of Paulownia fiber and its high-value application.

[0007] A green preparation method of paulownia fiber comprises the following steps: (1) Pretreatment of Paulownia bast: rinse the Paulownia bast with clean water to remove surface contamination, then soak the Paulownia bast in clean water for 24 to 48 hours and then dry it in an oven at a temperature of 50 to 60° C. for 2 to 3 hours to obtain the Paulownia bast after pretreatment; (2) Preparation of choline chloride DES: Choline chloride is used as the hydrogen bond acceptor of DES and mixed with a hydrogen bond donor in a molar ratio of 1:1 to 2, and heated at 80 to 100 °C until a clear and transparent low eutectic solvent is formed; (3) The pre-treated Paulownia bast obtained in step (1) is added to the low eutectic solvent obtained in the previous step in a certain mass ratio, and degummed at 140-160° C. for 1-2 h, and then the Paulownia fiber degummed with the low eutectic solvent is thoroughly washed with deionized water. The washing method is preferably suction filtration washing, and the filtrate is washed until the conductivity of the filtrate reaches ≤20 μS / cm, thereby obtaining Paulownia fiber.

[0008] The application of the Paulownia fiber obtained by the above method in the field of aerogel.

[0009] Furthermore, in the step (3), the mass ratio of the pre-treated Paulownia bast to DES is 1:20-100.

[0010] Furthermore, the hydrogen bond donor in step (2) is selected from at least one of urea, lactic acid and ethylene glycol.

[0011] The method for preparing cellulose micro-nano fiber aerogel by using the tung oil fiber prepared by the above method comprises the following steps: adding the tung oil fiber to deionized water, wherein the mass ratio of the tung oil fiber to the deionized water is 1:100-200, and mechanically degrading the tung oil fiber by using a high-speed shearing machine to decompose it into cellulose micro-nano fiber (CMNF for short); the speed of the high-speed shearing machine is 5000-10000 rpm, and the time is 10-15 min; after mechanical degradation, a CMNF dispersion is obtained; the concentration of the CMNF dispersion is adjusted to 5-6 mg / mL, and a cross-linking agent is added thereto, wherein the mass of the cross-linking agent in the dispersion is 5%-8% of the mass of the CMNF; the precursor dispersion is placed in a -60°C cold trap and frozen for 10-15 hours, and then transferred to a vacuum freeze dryer for drying, wherein the drying temperature is -60°C, the drying time is 48-72 hours, and after freeze drying, it is placed in a vacuum oven and heated at 100-120°C for 3-5 hours to complete cross-linking, thereby obtaining the CMNF aerogel.

[0012] Furthermore, the crosslinking agent is a polyamide epichlorohydrin resin, and the high-speed shearing machine is a wall breaker or a high-speed disperser, preferably an Aux household wall breaker or an Aika high-speed disperser.

[0013] The above-mentioned CMNF aerogel recovery method is to mix the used CMNF aerogel prepared above with deionized water, re-form a uniform CMNF dispersion under high-speed mechanical stirring, and then re-prepare the recovered CMNF aerogel product by freeze-drying, wherein the mechanical stirring adopts one of a household wall breaking machine or a high-speed disperser, the rotation speed is 5000-10000rpm, and the stirring time is 3-5min.

[0014] The above CMNF degradation method is to subject the above prepared CMNF glue to biodegradation treatment, wherein the biodegradation treatment method is a direct soil burial method.

[0015] Beneficial effects of the present invention: The present invention discloses a green preparation method of tung oil fiber, and provides a method for preparing tung oil bast fiber based on a one-step degumming process of DES, wherein different choline chloride DES are used to degumming tung oil bast, wherein the chloride ions in DES compete with the hydroxyl groups in carbohydrates and lignin to form hydrogen bonds, thereby destroying the chemical bonds between the lignin-carbohydrate complex and weakening the strong hydrogen bond interaction in the tung oil bast fiber. In addition, the protons (H+) separated from the DES hydrogen bond donor can catalyze the cleavage of the ether bonds and ester bonds of lignin and hemicellulose in the colloid component, so that lignin and hemicellulose are decomposed into small molecules, which are easy to dissolve in the solvent. Therefore, choline chloride DES can effectively remove the colloid components on the surface of tung oil fiber, and has the advantages of short process, high efficiency and energy saving, and high fiber production rate. In addition, the choline chloride DES used in the present invention belongs to a green solvent, has the advantages of low cost, easy preparation and recyclability, and is non-toxic, harmless, and biodegradable. Compared with all the strong acids and strong bases in traditional chemical degumming, there is no pollution and zero emission in the one-step degumming process of DES.

[0016] The tung oil fiber after DES degumming is mainly cellulose, with a multi-scale hierarchical structure composed of microfibers, nanofibers and graded cellulose chains. It should be noted that during the degumming of tung oil bast, DES can penetrate into the amorphous region of tung oil fiber, swell the fiber and weaken the hydrogen bonds and hydrophobic interactions between cellulose micro-nano fibers. Therefore, another object of the present invention is to further mechanically degrade the tung oil fiber treated with DES degumming into cellulose micro-nano fibers (CMNF for short) by simple mechanical treatment, and prepare functional materials such as CMNF aerogel by freeze-drying and other processes to achieve its high-value application. The CMNF aerogel prepared by the present invention belongs to biomass aerogel, which not only has the advantages of biodegradability and recyclability, but also shows excellent mechanical elasticity compared with traditional regenerated cellulose aerogel, and has broad application prospects in thermal insulation and environmental remediation. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The present invention is described in detail below with reference to the accompanying drawings. Figure 1 The results of the three choline chloride DES on (a) fiber production rate and (b) residual glue rate of Paulownia truncatum bast in Example 1; Figure 2The following are SEM images of Paulownia fiber before and after DES degumming in Example 1: (a) Paulownia bast fiber raw material; (b) Paulownia fiber degummed by choline chloride / ethylene glycol type DES; (c) Paulownia fiber degummed by choline chloride urea type DES; (d) Paulownia fiber degummed by choline chloride / lactic acid type DES; Figure 3 is the FTIR spectrum of the Paulownia fiber before and after CU-type DES degumming in Example 1; Figure 4 is the XRD spectrum of the Tong fiber before and after degumming by choline chloride urea type DES in Example 1; Figure 5 Schematic diagram of the degumming mechanism of Paulownia fiber by choline chloride urea type DES in Example 1; Figure 6 are (a) CMNF dispersion, (b) SEM image and (c) diameter distribution of CMNF prepared by high-speed mechanical degradation in Example 2; Figure 7 is the XRD spectra of degummed Paulownia fiber and CMNF in Example 2; Figure 8 The CMNF aerogel prepared in Example 2 is a photo of the CMNF aerogel: (a) an optical photo of the CMNF aerogel; (bc) a SEM image of the CMNF aerogel; (d) a flexible display of the CMNF aerogel; Fig. 9 (af) Optical photographs of the degradation of CMNF aerogels over time in Example 2; (gh) Optical photographs of yellow and black fungi on the surface of CMNF aerogels after 35 days of degradation; (i) Mass change of CMNF aerogels after 42 days of degradation; Fig.10 (af) are optical photographs of the degradation of the comparative polyethylene foam material over time in Example 2; Fig.11 This is a schematic diagram of the CMNF aerogel recovery process in Example 2. Fig.12 are optical photographs of the CMNF dispersion in Example 4 and SEM images of CMNF, wherein (a) is an optical photograph of the CMNF dispersion in Example 4; (bc) is a SEM image of CMNF; Fig.13 are SEM images of the CMNF aerogel in Example 4, where (ab) are SEM images of the CMNF aerogel at different magnifications. DETAILED DESCRIPTION

[0018] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1

[0019] Raw materials and equipment: Choline chloride (analytical grade), urea (analytical grade), lactic acid (90%), and ethylene glycol (analytical grade) were all purchased from Shanghai MacLean Biochemical Technology Co., Ltd.; the raw material of Tung tung bast was provided by Guizhou Jintong Ecological Agriculture Technology Co., Ltd.

[0020] The raw material of Paulownia tung oil was rinsed with clean water and soaked in it for 24 hours, and then the Paulownia tung oil fiber bundle was obtained by manual tearing, and the fiber bundle was dried at 60°C for 2 hours for standby use; choline chloride was mixed with urea, lactic acid and ethylene glycol respectively, and heated at 100°C until clear and transparent choline chloride / urea type, choline chloride / lactic acid type, and choline chloride / ethylene glycol type DES were formed, wherein the molar ratio of choline chloride to urea, lactic acid and ethylene glycol was 1:2; the Paulownia tung oil raw material was added to the three choline chloride DES prepared above, the mass ratio of fiber to DES was 1:20, and it was treated at 140°C for 2 hours. After completion, the degummed Paulownia tung oil fiber was filtered and washed until the conductivity of the washed filtrate was ≤20μS / cm, indicating that the residual DES was removed. It was further dried at 50°C to obtain degummed Paulownia tung oil fiber.

[0021] According to the previous research results of the research group (Li Changlong, Liu Qiong, Sun Ruixia, Wang Zongqian*. Chemical degumming and fiber performance analysis of Paulownia chinensis bast [J]. Journal of Textile Research, 2013, 34 (12): 8-11.), Paulownia chinensis bast mainly contains cellulose with a content of more than 65%, which is a plant fiber with high development value. The content of hemicellulose and lignin is higher than that of flax and ramie, so the degumming process of Paulownia chinensis bast fiber is relatively difficult. Although the research group previously adopted a two-boiling process combining acid pretreatment and caustic soda, which achieved good degumming effect and obtained Paulownia chinensis bast fiber with a low residual glue rate (4.2%), the process is long, energy-intensive and polluting. Therefore, the patent of this invention proposes a one-step degumming process based on choline chloride DES. Three different types of DES, namely choline chloride urea (CU), choline chloride / lactic acid (CL) and choline chloride / ethylene glycol (CE), were used to degumming Paulownia tung bast. The residual glue rate and fiber yield of the three DES were tested. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that among the three types of DES, the fiber yield rate (68.4%) and the residual glue rate (9.83%) of Paulownia tung oil fiber degumming by CE type DES were the lowest, while the fiber yield rate and residual glue rate of CU type DES were 72.8% and 3.03%, respectively, which were comparable to those of CL type (fiber yield rate: 74.2%, residual glue rate: 3.24%). SEM was further used to analyze the microstructure of Paulownia tung oil fiber after degumming with different DES. Figure 2 As can be seen from a, the surface of the undegummed Paulownia bast fiber is covered with colloid components, and the fiber surface is relatively rough. For CE-type DES, due to the limited ability of ethylene glycol in DES to remove hemicellulose and lignin in the colloid components, some colloid components still remain on the surface of Paulownia fiber ( Figure 2b), resulting in a high residual glue rate. In contrast, the surface of the Paulownia fiber treated with CU-type DES degumming is relatively smooth, with almost no residual glue ( Figure 2 c). This is mainly because the urea component in DES can destroy the hydrogen bond network between cellulose, hemicellulose and lignin, playing a key role in the dissolution process. The mild and effective action of CU-type DES ensures that non-cellulose impurities are effectively removed while retaining the structure of cellulose. It is worth noting that although the tung oil fiber prepared by CL-type DES degumming has a lower residual glue rate and a higher fiber yield, the acidic DES may cause partial damage to the tung oil fiber ( Figure 2 d).

[0022] Table 1. Mechanical properties of Paulownia fiber after different DES degumming treatments

[0023] The mechanical properties of the Paulownia fiber after degumming with three types of DES were further tested, and the results are shown in Table 1. As shown in Table 1, the fiber treated with CU-type DES has higher breaking strength and linear density values, which are 5.31±0.08cN / dtex and 6.11±0.1dtex, respectively, which meets the strength (grade 2 ≥4.00cN / dtex) and linear density (grade 3 ≤8.33dtex) grade indicators of the fiber in the Chinese National Standard for Textiles (GB / T20793-2015). After degumming with CL-type DES, the mechanical properties of Paulownia fiber (breaking strength 3.40±0.07cN / dtex, linear density 7.03±0.1dtex, elongation at break 1.09±0.05%) are lower than those of other samples, which is mainly because the acidic CL-type DES damages the structure of Paulownia fiber. In summary, the CE type DES has a poor effect on the degumming of Paulownia tung oil bark, while the CU type DES has the best degumming effect on Paulownia tung oil bark, which can effectively remove the colloid on the fiber surface without damaging the fiber. Although the CL type DES degumming has the lowest residual glue rate and the highest fiber yield of Paulownia tung oil fiber, it will cause partial damage to the fiber; it is worth noting that the partial damage caused by the CL type DES to the Paulownia tung oil fiber degumming will help to decompose it into cellulose micro-nanofibers through subsequent mechanical treatment.

[0024] The chemical structure changes of Paulownia fiber before and after CU-type DES degumming were tested by FTIR. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that the fibers of the Paulownia chinensis before and after degumming are both at 3427cm -1 The characteristic absorption peak at 1638cm corresponds to the -OH stretching vibration absorption peak in cellulose and lignin. However, the absorption intensity of this peak decreases significantly after degumming, indicating that the hydroxyl content decreases, which may be related to the removal of lignin during the degumming process.-1 and 1328cm -1 The absorption peaks at 1049cm are characteristic peaks of lignin. The absorption intensity of these two characteristic peaks of the Tong fiber decreased significantly after degumming, indicating that most of the lignin was removed after CU-type DES degumming. -1 and 900cm -1 The absorption peak at is related to natural hemicellulose. After degumming, the intensity of the absorption peak decreases or disappears, indicating that hemicellulose is removed during the degumming process. The changes in the crystal structure of the Paulownia fiber before and after degumming were further analyzed by X-ray diffraction spectroscopy (XRD). Figure 4 It can be seen that the Paulownia fiber before and after degumming has characteristic diffraction peaks at 15.2°, 16.6°, 22.7° and 34.5°, which belong to the (1-10), (110), (200) and (004) lattices, respectively. This shows that the CU-type DES degumming treatment does not destroy the structure of cellulose in the fiber, and the component still maintains the cellulose I crystal structure. In addition, according to the XRD spectrum, the crystallinity of the Paulownia fiber after degumming is 70.12%, which is higher than that of the undegummed Paulownia bast (64.9%), indicating that the CU-type DES degumming treatment removes the colloid component.

[0025] Based on the analysis results of FTIR and XRD, we proposed the degumming mechanism of Paulownia tung bast by DES. Figure 5 It can be seen that the chloride ions in DES compete with the hydroxyl groups in carbohydrates and lignin to form hydrogen bonds, thereby destroying the chemical bonds between the lignin-carbohydrate complex and weakening the strong hydrogen bonds between the Tung oil fibers. In addition, the protons (H + ) as a catalyst, which can catalyze the cleavage of ether and ester bonds in lignin and hemicellulose, so that lignin and hemicellulose are broken down into small molecules that are easily dissolved in DES. Therefore, the initially clear and transparent CU-type DES turns reddish brown after degumming. This color change is attributed to the dissolution of pectin, lignin, hemicellulose and other low molecular weight polymers in DES. Example 2

[0026] Raw materials and equipment: Oaks household wall-breaking machine HX-PB965B; polyamide epichlorohydrin resin (12%) was provided by Chengdu Aikoda Chemical Reagent Co., Ltd.; soil was taken from the top 20 cm soil of Yingyue Bridge Flower Field, Anhui University of Technology, Beijing Middle Road, Wuhu City, pH 7.14, and soil total organic carbon (TOC) content was (18.13±0.34) g kg -1 , moisture content is 50% of the total water retention capacity, stored in an insulated container at 4°C before use, without the use of pesticides or sterilization treatment.

[0027] In Example 1, the tung oil fiber degummed by CL (choline chloride / lactic acid) type DES was added into deionized water (the mass ratio of fiber to deionized water was 1:100), and mechanically degraded for 15 min at 5000 rpm using an Aux household wall-breaking machine to prepare a CMNF dispersion with a concentration of 5 mg / mL; a crosslinking agent polyamide epichlorohydrin resin was added to the above dispersion, and the mass of the crosslinking agent in the dispersion was 8% of the CMNF; the dispersion was poured into a Teflon mold and frozen at -60°C for 10 h, and then transferred to a vacuum freeze dryer for freeze drying (time: 48 h, cold trap temperature: -60°C) to obtain CMNF aerogel; finally, the aerogel was placed in a vacuum oven and heated at 120°C for 3 h to complete crosslinking.

[0028] Figure 6 The optical photo of CMNF dispersion formed by high-speed mechanical degradation and the SEM image and diameter distribution of CMNF. After high-speed mechanical blending, the degummed Paulownia fiber can be easily structured into CMNF ( Figure 6 a and b), compared with degummed Paulownia fiber ( Figure 2 c), the diameter of CMNF formed by mechanical degradation is significantly reduced, and its average diameter is 8.65 μm ( Figure 6 c), the length exceeds 800 μm ( Figure 6 b) has a high aspect ratio, which confirms that the strong Paulownia fiber can maintain its high aspect ratio during mechanical treatment. The degummed Paulownia fiber and CMNF aggregate structure were analyzed by XRD spectra. Figure 7 As shown in the figure, it can be seen that both of them have characteristic diffraction peaks at 2θ=15.2°, 16.6° and 22.2°, corresponding to the (10), (110) and (200) crystal planes of cellulose Iβ, respectively; in addition, the positions of the characteristic diffraction peaks of degummed tung oil bast fiber and CMNF have not changed, indicating that the mechanical treatment has not destroyed the aggregated structure of cellulose, which is conducive to the subsequent construction of highly elastic aerogel functional materials as assembly units.

[0029] CMNF aerogels were further prepared by freeze drying, such as Figure 8 As shown in a, the aerogel has ultra-light properties and a density as low as 8.3 mg / cm 3 , and can stand on the foxtail grass seed hair without bending it. SEM morphology shows that CMNF aerogel is assembled by entanglement of interconnected CMNFs and has a highly porous structure ( Figure 8 bc), this unique microstructure gives CMNF aerogel good flexibility. Figure 8 As shown in Figure d, the CMNF aerogel is folded approximately 180° without breaking it, and the aerogel can return to its original shape after being released.

[0030] In order to evaluate the biodegradability of CMNF aerogel materials, they were buried in soil and their morphology and weight changes were observed regularly. Fig. 9 As shown in af, as the time of burial in soil increases, the CMNF aerogel gradually degrades. After 14 days of burial in soil, the foaming material began to change. After 35 days, a large number of yellow and black fungi appeared on the surface of CMC aerogel material ( Fig. 9 g and h). After 46 days, CMNF was completely degraded. In addition, after 42 days, the dry weight of the foamed material decreased from 1.22 g to 0.14 g, indicating that about 88.5% of the CMNF aerogel was degraded ( Fig. 9 i). In contrast, the morphology of polyethylene foam material changed after being buried in the soil for 46 days ( Fig.10 ). These results show that the biodegradability of cellulose foam materials is better than that of traditional polyethylene foam materials. More importantly, CMNF aerogels are recyclable. CMNF aerogels at the end of their service life can be mixed with deionized water to form a CMNF dispersion through simple mechanical stirring, and CMNF aerogels can be re-prepared by freeze drying ( Fig.11 ). Therefore, the aerogel material prepared from Tung oil fiber is expected to replace the traditional petroleum-based polymer aerogel due to its cost-effectiveness, biodegradability and non-toxicity, recyclability and high elasticity, and has broad application prospects in the fields of thermal insulation and environmental treatment. Example 3

[0031] Raw materials and equipment: Choline chloride and urea were of analytical grade and provided by Shanghai MacLean Biochemical Technology Co., Ltd.; the raw material of Paulownia scoparia was provided by Guizhou Jintong Ecological Agriculture Technology Co., Ltd.

[0032] The raw material of Paulownia bast was rinsed with clean water and soaked in it for 48 hours, and then the Paulownia bast fiber bundle was obtained by manual tearing, and the fiber bundle was dried at 50°C for 3 hours for standby use; choline chloride was mixed with urea and heated at 80°C until a clear and transparent choline chloride / lactic acid type DES was formed, wherein the ratio of choline chloride to urea was 1:2; the Paulownia bast raw materials were added to the choline chloride / lactic acid type DES prepared above, and the mass ratio of fiber to DES was 1:100, and treated at 160°C for 1 hour. After completion, the degummed Paulownia fiber was filtered and washed until the conductivity of the washed filtrate was ≤20μS / cm, indicating that the residual DES was removed. The degummed Paulownia fiber was obtained and further dried at 50°C for 2 hours. Example 4

[0033] Raw materials and equipment: Aika T25 high-speed disperser; polyamide epichlorohydrin resin is provided by Guangxi Guitang Group Co., Ltd.

[0034] The Paulownia fiber obtained in Example 3 was added to deionized water (the mass ratio of fiber to deionized water was 1:200), and mechanically degraded for 10 min at 10000 rpm using a high-speed disperser to prepare a CMNF dispersion with a concentration of 6 mg / mL; a crosslinking agent polyamide epichlorohydrin resin was added to the above dispersion, and the mass of the crosslinking agent in the dispersion was 5% of the CMNF; the dispersion was poured into a Teflon mold and frozen at -60°C for 15 h, and then transferred to a vacuum freeze dryer for freeze drying (time: 72 h, cold trap temperature: -60°C) to obtain CMNF aerogel; finally, the aerogel was placed in a vacuum oven and heated at 100°C for 5 h to complete crosslinking.

[0035] The photograph of the CMNF dispersion prepared by mechanical treatment in Example 4 and the SEM morphology of CMNF are shown in Fig.12 As shown, it can be seen that the CMNF dispersion is uniform and stable ( Fig.12 a), SEM images show that the diameter of CMNF is about 10 μm, and there are nanoscale cellulose fibrils on the surface of cellulose microfibers ( Fig.12 bc). Fig.13 It can be seen that the CMNF aerogel prepared in Example 4 is also assembled by entanglement of CMNF ( Fig.13 a), and the CMNFs are bonded by cross-linking agent polyamide epichlorohydrin resin ( Fig.13 b).

Claims

1. A green preparation method of Paulownia tung oil fiber, characterized in that: The following steps are involved: (1) Pretreatment of Paulownia tung bast: rinse the Paulownia tung bast with clean water, soak the Paulownia tung bast in clean water for 24 to 48 hours, and then dry it in an oven at a temperature of 50 to 60° C. for 2 to 3 hours to obtain the Paulownia tung bast after pretreatment; (2) Preparation of choline chloride-based low eutectic solvents: Choline chloride is used as a hydrogen bond acceptor of the low eutectic solvent and mixed with a hydrogen bond donor in a molar ratio of 1:1 to 2, and heated at 80 to 100° C. until a clear and transparent low eutectic solvent is formed; (3) The pre-treated Paulownia bast obtained in step (1) is added to the low eutectic solvent obtained in the previous step in a certain mass ratio, and degummed at 140-160° C. for 1-2 h, and then the Paulownia fiber degummed with the low eutectic solvent is thoroughly washed with deionized water until the conductivity of the filtrate reaches ≤20 μS / cm, thereby obtaining Paulownia fiber.

2. The green preparation method of Paulownia fiber according to claim 1, characterized in that: In the step (3), the mass ratio of the pre-treated Paulownia truncatum bast to the low eutectic solvent is 1:20-100.

3. The green preparation method of Paulownia fiber according to claim 1, characterized in that: The hydrogen bond donor in step (2) is selected from at least one of urea, lactic acid and ethylene glycol.

4. Application of the Paulownia fiber obtained according to the preparation method according to any one of claims 1 to 3 in the field of aerogel.

5. A method for preparing cellulose micro-nano fiber aerogel using the Paulownia fiber prepared by the method of claim 1, characterized in that: The method comprises the following steps: adding tung oil fiber into deionized water, wherein the mass ratio of tung oil fiber to deionized water is 1:100-200, and mechanically degrading the tung oil fiber by a high-speed shearing machine to decompose the tung oil fiber into cellulose micro-nano fiber; the rotation speed of the high-speed shearing machine is 5000-10000 rpm, and the time is 10-15 minutes; after mechanical degradation, a cellulose micro-nano fiber dispersion is obtained; the concentration of the cellulose micro-nano fiber dispersion is adjusted to 5-6 mg / mL, and a cross-linking agent is added thereto, wherein the mass of the cross-linking agent in the dispersion is 5%-8% of the mass of the cellulose micro-nano fiber; placing the precursor dispersion in a -60°C cold trap for freezing for 10-15 hours, and then transferring it to a vacuum freeze dryer for drying treatment, wherein the drying treatment temperature is -60°C, the drying time is 48-72 hours, and after freeze drying, placing it in a vacuum oven and heating it at 100-120°C for 3-5 hours to complete cross-linking, thereby obtaining a cellulose micro-nano fiber aerogel.

6. The method for preparing cellulose micro-nano fiber aerogel according to claim 4, characterized in that: The cross-linking agent is polyamide epichlorohydrin resin, and the high-speed shearing machine is a household wall-breaking machine or a high-speed disperser.

7. Cellulose micro-nano fiber aerogel prepared by the preparation method according to any one of claims 5 to 6.

8. A method for recovering cellulose micro-nanofiber aerogel, characterized in that: The cellulose micro-nano fiber aerogel according to claim 7 after use is mixed with deionized water, and a uniform cellulose micro-nano fiber aerogel dispersion is re-formed under the action of high-speed mechanical stirring, and then the recycled cellulose micro-nano fiber aerogel product is re-prepared through freeze-drying, wherein the mechanical stirring adopts one of a household wall-breaking machine or a high-speed disperser, the rotation speed is 5000-10000rpm, and the stirring time is 3-5min.

9. A method for degrading cellulose micro-nanofiber aerogel, characterized in that: The cellulose micro-nano fiber aerogel according to claim 7 is subjected to biodegradation treatment, wherein the biodegradation treatment is a direct soil burial method.

Citation Information

Cited By

  • Ternary eutectic solvent for dissolving cellulose as well as preparation method and use method of ternary eutectic solvent

    CN121226780A