Microorganism-based composite nanofiber material loaded with nano silver phosphate as well as preparation method and application thereof
Nano silver phosphate composite fiber material formed by adsorption of microorganisms and silver ion solution and polymer spinning technology solves the high cost and easy loss problems of silver nanoparticles synthesis in the prior art, and achieves uniform distribution and efficient extraction of silver ions , suitable for solid phase extraction of complex samples.
Patent Information
- Application Number
- CN202411098827.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-08
AI Technical Summary
The synthesis of silver nanoparticles in existing composite nanomaterials has problems such as strict control of preparation conditions, high reagent consumption, low crystallinity, high energy consumption, high cost, and easy loss of silver and difficult to recover. Especially in silver solid phase extraction technology, The high price and easy loss of silver materials are difficult to solve.
Using microbial-based composite nanofiber materials with nano silver phosphate loading, the surface and internally loaded silver phosphate composites generated by adsorption of microorganisms and silver ion solutions are doped into the polymer spinning liquid, and electrospinning technology is used. The formation of porous composite nanofiber materials avoids agglomeration and growth of traditional physicochemical methods, and achieves uniform distribution and high affinity of silver ions.
It realizes low cost, easy storage and high dispersion of silver ions, avoids silver loss, improves the extraction rate and controllability of materials, and is suitable for the field of solid phase extraction, especially in the purification of unsaturated fatty acid methyl esters and biothiols. , enrichment and extraction showed high efficiency.
Smart Images

Figure CN118910755A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new material preparation, and relates to a composite nanofiber material loaded with nano silver phosphate based on microorganisms, and a preparation method and application thereof. Background Art
[0002] The extraction, separation and rapid detection of specific components in complex matrix samples are difficult problems that need to be overcome in the field of analytical chemistry. Silver solid phase extraction technology is a pretreatment technology that uses silver to extract certain specific structural substances in samples. At present, silver solid phase extraction materials generally include silver-containing single substances (Ag NPs), carriers loaded with silver ions (such as covalent organic polymers COP), or silver ion liquids (such as AgBF4), which have the disadvantages of high price, easy loss of silver and difficulty in recovery.
[0003] The synthesis of silver nanoparticles in existing composite nanomaterials is usually prepared by physical and chemical methods, which have shortcomings such as the need for strict control of preparation conditions, large reagent consumption, low crystallinity, high energy consumption, and high product cost. Summary of the invention
[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a composite nanofiber material based on microorganisms loaded with nano silver phosphate, which has low cost, is not easy to lose silver, is easy to preserve, and has a highly dispersed silver phosphate complex, and can avoid the agglomeration growth of crystals in the traditional physical and chemical synthesis process.
[0005] The technical problem that the present invention also aims to solve is to provide a method for preparing a composite nanofiber material based on microorganisms loaded with nano silver phosphate, which has readily available raw materials, a controllable preparation process and convenient operation.
[0006] The final technical problem to be solved by the present invention is to provide an application of the microorganism-based composite nanofiber material loaded with nano silver phosphate in solid phase extraction.
[0007] Technical solution: In order to solve the above technical problems, the present invention provides a composite nanofiber material based on microorganisms loaded with nano silver phosphate. The composite nanofiber material is a material loaded with silver phosphate complex on the surface and inside, which is generated by adsorbing microorganisms and silver ion solution and then doping it into a high molecular polymer spinning solution.
[0008] Wherein, the microorganisms include one or more of Pichia pastoris, Escherichia coli, Shewanella, Staphylococcus aureus or Bacillus subtilis.
[0009] Wherein, the silver ion solution is a silver nitrate solution or a silver borofluoride solution, and its silver ion concentration is ≥50 mg / L.
[0010] The polymer spinning solution includes a solute and a solvent. The solute is a polymer, including one or more of polyethylene oxide, polypyrrole, polyethylene naphthalate, polyaniline, nylon, polyphenylene sulfide, cellulose acetate, polystyrene, polycaprolactam, acrylic resin and polyacrylonitrile; the solvent includes one or more of ethyl acetate, N,N-dimethylformamide, tetrahydrofuran, formic acid, acetic acid, ethanol, acetone, water, halogenated hydrocarbons and aromatic hydrocarbons.
[0011] Preferably, the composite nanofiber material loaded with nano silver phosphate is in a fiber shape, and its diameter is 100 to 500 nm.
[0012] The present invention also provides a method for preparing the microorganism-based composite nanofiber material loaded with nano silver phosphate, comprising the following steps:
[0013] 1) The cultured microorganisms are broken, ultrasonically dispersed in distilled water for washing, precipitated or separated by high-speed centrifugation, and then freeze-dried in vacuum;
[0014] 2) adding the vacuum freeze-dried bacterial cells in step 1) into a silver ion solution for reaction, wherein the silver ions and the phosphate groups of the microorganisms are prepared into a silver phosphate complex, which is then allowed to settle or centrifuged and then vacuum freeze-dried;
[0015] 3) placing the silver phosphate complex synthesized by the microorganism in step 2) in a dissolved high molecular polymer spinning solution, mixing evenly and then performing electrostatic spinning to finally form a microorganism-based silver phosphate composite nanofiber material.
[0016] Wherein, the silver ion solution in step 2) comprises a silver nitrate solution, and the silver ion concentration is 50 to 400 mg / L.
[0017] Wherein, in step 2), the mass volume ratio of the bacteria to the silver ion solution is 0.1 g / L-10 g / L.
[0018] Wherein, in step 3), the mass volume ratio of the silver phosphate complex to the high molecular polymer spinning solution is 0.01 g / mL-1 g / mL.
[0019] Wherein, the voltage of the electrospinning in step 3) is 10-30 kV, the receiving distance is 10-20 cm, the flow rate is 0.5-2.5 mL / min, and the air humidity is 30-70%.
[0020] The present invention also provides the application of the microorganism-based composite nanofiber material loaded with nano silver phosphate in solid phase extraction.
[0021] The composite nanofiber material loaded with nano silver phosphate is used for solid phase extraction of unsaturated fatty acid methyl ester and biothiol.
[0022] Wherein, the unsaturated fatty acid methyl esters are oleic acid methyl ester, linoleic acid methyl ester, linolenic acid methyl ester, etc.; the biothiols include reduced glutathione, cysteine, homocysteine, etc.
[0023] Among them, the application includes loading the composite nanofiber material loaded with nano silver phosphate into the solid phase extractor shell, and after the sample solution completely flows through the bed of the composite nanofiber material loaded with nano silver phosphate, adding the corresponding eluent into the solid phase microextractor, and collecting the outflowing solution after the eluent flows through the bed of the composite nanofiber material loaded with nano silver phosphate. After the elution is completed, the sample is tested on the machine as soon as possible or frozen for testing.
[0024] The concentration of the unsaturated fatty acid and biothiol aqueous solution is 1-1000 μg / mL, the filling amount of the composite nanofiber material loaded with nano silver phosphate is 5-50 mg; and the eluent is ethyl acetate, mercaptoethanol, etc.
[0025] Mechanism of the present invention: The present invention uses broken microorganisms as a matrix, obtains a silver phosphate composite material by adsorbing silver ions, and obtains a porous composite nanofiber material after doping with a polymer material for spinning. The surface and interior of the composite nanofiber material are loaded with a silver phosphate composite, and have excellent adsorption characteristics for unsaturated fatty acid methyl esters and biological mercaptan. The broken microorganisms adsorb silver ions and then dope them into a polymer material for spinning to form a solid phase extraction material. The specific principle is that the microbial fragments are placed in a silver salt solution as an adsorbent, and the positively charged metal ions are adsorbed by the electronegative microorganisms under the action of electrostatics, and then the silver phosphate composite is generated. After the composite is freeze-vacuum dried, it is mixed with a polymer spinning solution for spinning, so that the silver phosphate composite is evenly distributed inside and on the surface of the nanofiber, thereby obtaining a composite nanofiber material loaded with nano silver phosphate. When the microorganisms adsorb metal ions, the active groups play a major role. After the microorganisms are broken, more functional groups are exposed, and the prepared nanofibers have potential applications in solid phase extraction of unsaturated fatty acid methyl esters and biological mercaptan.
[0026] Beneficial effects: Compared with the prior art, the advantages of the present invention are:
[0027] (1) Microorganisms contain many active groups and rich phosphorus sources. They can adsorb metal ions from metal salt solutions to form metal complexes. This technology avoids the addition of phosphates to complete the reaction and has the advantages of being green and environmentally friendly. Silver phosphate complexes are generated by adsorbing silver ions and then spun into polymer nanofibers, making it difficult for silver ions to be lost and easy to recover. The silver is evenly distributed and can be used for adsorption of target substances with a high extraction rate. The preparation process of this material is controllable and easy to operate, making it suitable for application in the field of solid phase extraction. Compared with conventional chemical synthesis methods, the silver in this material is not easy to be lost, is easy to preserve, and is easy to recycle after use. Moreover, the phosphorus source comes from microorganisms, which avoids the risk of phosphorus pollution from the phosphorus source and is green and environmentally friendly.
[0028] (2) The composite nanofiber material loaded with nano silver phosphate based on microorganisms disclosed in the present invention uses microorganisms with high affinity for silver ions as precursors to generate silver phosphate complexes in situ, and forms the composite nanofiber material through electrostatic spinning technology. The composite nanofiber material not only has the selective extraction properties of silver solid phase extraction materials, but also makes silver ions less likely to be lost due to its special composite composition structure. The composite nanofiber material of nano silver phosphate is loaded into a solid phase extractor and can be used for the purification, enrichment and extraction of unsaturated fatty acids and biothiols in various complex samples. The target substances obtained by extraction can be injected into analytical instruments for detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a scanning electron microscope image of the composite nanofiber material loaded with nano silver phosphate in Example 1.
[0030] Figure 2 This is the energy spectrum of the composite nanofiber material loaded with nano silver phosphate in Example 1.
[0031] Figure 3 It is the XRD diagram of the composite nanofiber material loaded with nano silver phosphate in Example 1, with the PDF card JCPDS 06-0505 corresponding to Ag3PO4.
[0032] Figure 4 This is a solid phase extraction effect diagram of three unsaturated fatty acid methyl esters in Example 2.
[0033] Figure 5 This is a scanning electron microscope image of the composite nanofiber material loaded with nano silver phosphate in Example 3.
[0034] Figure 6 It is the XRD pattern of the composite nanofiber material loaded with nano silver phosphate of Example 3, with the PDF card JCPDS 06-0505 corresponding to Ag3PO4.
[0035] Figure 7 This is a diagram showing the solid phase extraction effect of reduced glutathione in Example 4. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is further described below in conjunction with specific embodiments and drawings, but the protection scope of the present invention is not limited to the following specific embodiments.
[0037] Unless otherwise defined, all technical terms used hereinafter are identical with those skilled in the art generally understood. Technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. The extractor used in the embodiments of the present invention can be selected to use the extractor housing disclosed in Chinese Patent No. 2005101231485 or 201020500026X and the solid phase extractor housing without adsorbent of conventional size.
[0038] The composite nanofiber material loaded with nano silver phosphate based on microorganisms prepared in the present invention adopts microorganisms with high affinity for silver ions as precursors, generates silver phosphate complex in situ, and forms the composite nanofiber material through electrostatic spinning technology. It not only has the selective extraction property of silver solid phase extraction materials, but also makes silver ions difficult to lose due to its special composite composition structure. The composite nanofiber material of nano silver phosphate is loaded into a solid phase extractor, which can be used for the purification, enrichment and extraction of unsaturated fatty acids and biothiols in various complex samples, and the target obtained by extraction can be injected into an analytical instrument for detection.
[0039] Example 1 Preparation of composite nanofiber material loaded with nano silver phosphate based on Pichia pastoris
[0040] 1) Pichia pastoris X-33 cultured to maturity was centrifuged at 10,000 rpm, then ultrasonically disrupted for 60 min, and vacuum freeze-dried.
[0041] 2) Prepare a silver nitrate solution with a silver ion concentration of 500 mg / L. Add the dried Pichia pastoris X-33 to the prepared 500 mg / L silver ion solution to form a solution with a strain concentration of 2 g / L, and stir and adsorb at 25°C for 6 hours; then naturally settle, take the precipitate and vacuum freeze-dry for 8 hours to obtain a complex of Pichia pastoris fragments and silver phosphate;
[0042] 3) Using N,N-dimethylformamide as solvent, a 10% (wt%) polyacrylonitrile (PAN) solution was prepared, and 0.5 g of the Pichia fragments and the silver phosphate complex were placed in the 10% (wt%) PAN solution to form a spinning solution with a concentration of 5% (wt%) of the Pichia fragments and the silver phosphate complex, which was stirred evenly and ultrasonically dispersed for 30 minutes for standby use.
[0043] 4) Electrospinning was performed under the conditions of a voltage of 20 kV, a receiving distance of 10 cm, a flow rate of 1.2 mL / min, and an air humidity of 50% to prepare a composite nanofiber material in which the Pichia pastoris X-33 fragments and the silver phosphate complex were evenly dispersed.
[0044] Depend on Figure 1 It can be seen that the Pichia fragments and silver phosphate complex exist inside and outside the PAN fiber. The material is fibrous, with a fiber diameter of 100 to 300 nm and an average diameter of 170 nm. Figure 2 It can be seen that Ag3PO4 is evenly distributed in the PAN matrix. Figure 3 It can be seen that the XRD results of the prepared materials show that the diffraction peak of the composite nanofiber material loaded with nano silver phosphate corresponds to the diffraction peak of Ag3PO4 with the PDF card JCPDS 06-0505.
[0045] Example 2 Application of composite nanofiber materials loaded with nano-silver phosphate based on Pichia pastoris - Solid phase extraction of methyl oleate, methyl linoleate and methyl linolenate in aqueous solution
[0046] The composite nanofiber material prepared in Example 1 was applied to solid phase extraction in an unsaturated fatty acid aqueous solution with a concentration of 50 μg / mL, eluted with ethyl acetate, and then detected by gas chromatography. The specific steps are as follows:
[0047] 1. Prepare a certain concentration of methyl oleate, methyl linoleate and methyl linolenate stock solutions with methanol, dilute with distilled water to prepare methyl oleate, methyl linoleate and methyl linolenate aqueous solutions with a concentration of 50 μg / mL as sample solutions; dilute with methanol solution to prepare methanol solution standard solutions S0 with a concentration of 50 μg / mL of methyl oleate, methyl linoleate and methyl linolenate.
[0048] 2. Transfer 500 μL of the sample solution prepared in step 1 to a solid phase microextractor filled with an extraction column of a composite nanofiber material loaded with nano-silver phosphate based on Pichia yeast prepared in Example 1. After the sample solution has completely flowed through the nanofiber column bed, transfer 500 μL of ethyl acetate eluent to the solid phase microextractor. After the eluent has flowed through the nanofiber column bed, collect the outflowing solution. After the elution is completed, test it on the machine as soon as possible or freeze the sample for testing.
[0049] Figure 4The extraction effect of composite nanofiber material loaded with nano silver phosphate on methyl oleate, methyl linoleate and methyl linolenate in aqueous solution, methyl oleate, methyl linoleate and methyl linolenate peak at 16.43min, 17.53min and 19.07min respectively, the prepared extraction column has a good extraction effect on unsaturated fatty acid methyl ester, the extraction efficiency is 104.8%, 96.5% and 108.3% respectively. The calculation formula is as follows:
[0050] Extraction efficiency = (S / S0) * 100%
[0051] S is the peak area of fatty acid methyl esters in the eluate after solid phase extraction, and S0 is the peak area of the methanol standard solution of fatty acid methyl esters without solid phase extraction.
[0052] Example 3 Preparation of composite nanofiber material loaded with nano silver phosphate based on Escherichia coli
[0053] 1) The mature Escherichia coli BL 21 cultured for 72 hours was centrifuged at 12000 rpm, then ultrasonically disrupted for 120 minutes, and vacuum freeze-dried.
[0054] 2) preparing a silver nitrate solution with a silver ion concentration of 400 mg / L, placing the dried Escherichia coli BL 21 fragments in the prepared silver ion solution to form a solution with a bacterial concentration of 2 g / L, and stirring and adsorbing at 25° C. for 12 hours; then naturally settling, taking the precipitate and vacuum freeze-drying it for 8 hours to obtain a complex of Escherichia coli BL 21 fragments and silver phosphate.
[0055] 3) Using a mixed solution of tetrahydrofuran and N,N-dimethylformamide (6:4 / v:v) as solvent, prepare 10%
[0056] (wt%) polystyrene (PS) solution, 0.4 g of E. coli fragments and silver phosphate complex were placed in a 10%
[0057] A mixed spinning solution with a bacterial concentration of 4% (wt%) was formed in a (wt%) polystyrene (PS) solution, which was stirred evenly and ultrasonically dispersed for 120 minutes for standby use.
[0058] 4) Electrospinning was performed under the conditions of a voltage of 25 kV, a receiving distance of 12 cm, a flow rate of 1.0 mL / min, and an air humidity of 70% to prepare a composite nanofiber material in which the Escherichia coli BL 21 fragments and the silver phosphate complex were evenly dispersed.
[0059] Depend on Figure 5 It can be seen that the material prepared in this example has a fibrous morphology, and the E. coli fragments and the silver phosphate complex exist inside and outside the PS fiber. The fiber diameter is 100-400 nm, and the average diameter is 241 nm.
[0060] Depend on Figure 6 It can be seen that the XRD results of the prepared materials show that the diffraction peak of the composite nanofiber material loaded with nano silver phosphate corresponds to the diffraction peak of Ag3PO4 with the PDF card JCPDS 06-0505.
[0061] Example 4 Rapid extraction and separation of reduced glutathione from aqueous solution using composite nanofiber material loaded with nano-silver phosphate based on Escherichia coli
[0062] The material prepared in Example 3 was applied to the solid phase extraction of reduced glutathione in a 10 μg / mL aqueous solution, eluted with an 8% mercaptoethanol methanol solution, derivatized with 0.1 mol / L OPA (pH=9) in a phosphate buffer, and then detected by liquid chromatography. The specific steps are as follows:
[0063] 1. Preparation of reduced glutathione in aqueous solution
[0064] A certain concentration of reduced glutathione stock solution was prepared with distilled water, and diluted with distilled water to prepare a reduced glutathione aqueous solution with a concentration of 10 μg / mL, which was the standard solution S0 and the sample solution.
[0065] 2. Solid phase extraction of reduced glutathione from aqueous solution
[0066] The 200 μL sample solution of step 1 was transferred to a solid phase microextractor filled with the composite nanofiber material based on Escherichia coli loaded with nano-silver phosphate prepared in Example 3, and after the sample solution completely flowed through the nanofiber column bed. Then 200 μL of 8% mercaptoethanol methanol solution eluent was transferred to the solid phase microextractor, and after the eluent flowed through the nanofiber column bed, the outflow solution was collected, and then derivatized with 200 μL of 0.1 mol / L OPA (pH=9) phosphate buffer, and tested on the machine.
[0067] Figure 7 The composite nanofiber material loaded with nano-silver phosphate based on Escherichia coli is used to extract reduced glutathione in aqueous solution. The reduced glutathione peaks at 6.99 min. The material has a good effect on the solid phase extraction of reduced glutathione, and the extraction efficiency is 102.2%.
[0068] Extraction efficiency = (S / S0) * 100%
[0069] S is the peak area of reduced glutathione in the eluate after solid phase extraction, and S0 is the peak area of the standard solution of reduced glutathione standard dissolved in water without solid phase extraction.
Claims
1. Composite nanofiber materials loaded with nano silver phosphate based on microorganisms, It is characterized in that The composite nanofiber material is a material with silver phosphate complex loaded on the surface and inside, which is generated by adsorbing microorganisms and silver ion solution and then doping into a high molecular polymer spinning solution.
2. The microorganism-based composite nanofiber material loaded with nano silver phosphate according to claim 1, It is characterized in that The microorganisms include one or more of Pichia pastoris, Escherichia coli, Shewanella, Staphylococcus aureus or Bacillus subtilis.
3. The microorganism-based composite nanofiber material loaded with nano silver phosphate according to claim 1, It is characterized in that The silver ion solution is a silver nitrate solution or a silver borofluoride solution, and its silver ion concentration is ≥50 mg / L.
4. The microorganism-based composite nanofiber material loaded with nano silver phosphate according to claim 1, It is characterized in that The high molecular polymer spinning solution includes a solute and a solvent. The solute is a high molecular polymer, including one or more of polyethylene oxide, polypyrrole, polyethylene naphthalate, polyaniline, nylon, polyphenylene sulfide, cellulose acetate, polystyrene, polycaprolactam, acrylic resin and polyacrylonitrile; the solvent includes one or more of ethyl acetate, N,N-dimethylformamide, tetrahydrofuran, formic acid, acetic acid, ethanol, acetone, water, halogenated hydrocarbons and aromatic hydrocarbons.
5. The method for preparing the composite nanofiber material loaded with nano silver phosphate based on microorganisms according to any one of claims 1 to 4, It is characterized in that The following steps are involved: 1) Crush the cultured microorganisms, disperse them in distilled water with ultrasonic wave, wash them, separate solid and liquid by precipitation or high-speed centrifugation, and then freeze-dry them in vacuum; 2) adding the vacuum freeze-dried bacterial cells in step 1) into a silver ion solution for reaction, wherein the silver ions and the phosphate groups of the microorganisms are prepared into a silver phosphate complex, which is then allowed to settle or centrifuged and then vacuum freeze-dried; 3) placing the silver phosphate complex synthesized by the microorganism in step 2) in a dissolved high molecular polymer spinning solution, mixing evenly and then performing electrostatic spinning to finally form a microorganism-based silver phosphate composite nanofiber material.
6. The method for preparing the composite nanofiber material loaded with nano silver phosphate based on microorganisms according to claim 5, It is characterized in that The silver ion solution in step 2) includes a silver nitrate solution, and the silver ion concentration is 50-400 mg / L.
7. The method for preparing the composite nanofiber material loaded with nano silver phosphate based on microorganisms according to claim 5, It is characterized in that In step 2), the mass volume ratio of the bacteria to the silver ion solution is 0.1 g / L-10 g / L.
8. The method for preparing the composite nanofiber material loaded with nano silver phosphate based on microorganisms according to claim 5, It is characterized in that In step 3), the mass volume ratio of the silver phosphate complex to the high molecular polymer spinning solution is 0.01 g / mL-1 g / mL.
9. The method for preparing the composite nanofiber material loaded with nano silver phosphate based on microorganisms according to claim 5, It is characterized in that The voltage of the electrospinning in step 3) is 10 ~ 30 kV, the receiving distance is 10 ~ 20 cm, the flow rate is 0.5 ~ 2.5 mL / min, and the air humidity is 30 ~ 70%.
10. Use of the microorganism-based composite nanofiber material loaded with nano silver phosphate as described in any one of claims 1 to 4 in solid phase extraction.