Antibacterial acarus-killing polyester blended wool fabric and preparation method thereof

By using carbon quantum dot/nanosilver/porous silica microsphere composite materials in polyester blended wool fabrics, the dispersion and compatibility problems of nanosilver in fibers are solved, and the antibacterial mite removal performance and fiber strength are improved. Achieve high-quality polyester blended wool fabric.

CN118910781AInactive Publication Date: 2024-11-08HANGZHOU ZHONGJUN TECH CO LTD

Patent Information

Application Number
CN202411219561.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When existing polyester blended wool fabrics absorb nano silver, they are not dispersible and have poor compatibility with fibers, which affects fiber strength and antibacterial and mite removal performance.

Method used

Carbon quantum dots/nanosilver/porous silica microsphere composite material is used as the additive for modified polyester fibers, and carbon quantum dots and nanosilver are loaded through porous silica microspheres as carriers, and polyethylene glycol and silane are added to couple The agent improves its dispersion and compatibility in the fibers, and combines the ethylene-acrylate-maleic anhydride terpolymer to prepare a polyester blended wool fabric with excellent antibacterial and mite removal performance.

Benefits of technology

It realizes the high antibacterial properties and anti-mites of polyester blended wool fabrics, while improving the strength of the fibers, ensuring product quality and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of textile, in particular to an antibacterial and acarus-killing polyester blended wool fabric and a preparation method thereof.The antibacterial and acarus-killing polyester blended wool fabric is prepared from, by weight, 50-70 parts of modified polyester fibers and 30-50 parts of wool; the modified polyester fiber is prepared from the following raw materials: polyester, a carbon quantum dot / nano-silver / porous silicon dioxide microsphere composite material and an ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of the polyester to the carbon quantum dot / nano-silver / porous silicon dioxide microsphere composite material to the ethylene-acrylate-maleic anhydride terpolymer is 100: (3.5-5): (3-6); the polyester blended wool fabric disclosed by the invention has excellent antibacterial property and mite prevention and removal performance, and the used polyester fibers are high in strength, so that the product quality of the obtained polyester blended wool fabric can be effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to an antibacterial and mite-removing polyester blended wool fabric and a preparation method thereof. Background Art

[0002] Polyester blended wool fabric refers to a fabric made by mixing polyester fiber and wool fiber in a certain proportion. Polyester blended wool fabric has good dimensional stability and corrosion resistance, is easy to wash and dry, has good wrinkle recovery, and is moderately priced. It is favored by consumers and its application is becoming more and more extensive. At present, children's plush toys, pet carpets, etc. are also mostly made of polyester blended wool fabric.

[0003] The materials and structures of plush toys and carpets easily absorb dust, dandruff and other pollutants, providing an ideal breeding environment for bacteria and mites. In addition, plush toys for children are easily contaminated with children's sweat, saliva and other secretions, further increasing the risk of bacteria and mites breeding. In order to reduce the potential threat of plush toys and carpets to the health of children and pets, it is necessary to use polyester blended wool fabrics with antibacterial and mite-removing properties to prepare plush toys and carpets.

[0004] Since nanosilver has strong antibacterial ability, it is often used to modify the antibacterial and mite removal performance of fabrics. In order to make the antibacterial effect more lasting, nanosilver is often added as an additive to fiber-forming polymers for spinning. However, nanosilver has poor dispersion in fibers and poor compatibility with fibers, which reduces the strength of the fibers and affects the quality of polyester blended wool fabrics. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide an antibacterial and mite-removing polyester blended wool fabric and a preparation method thereof. The polyester blended wool fabric has excellent antibacterial and anti-mite and mite-removing properties, and the polyester fiber used has high strength, which can effectively ensure the product quality of the obtained polyester blended wool fabric.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 50-70 parts of modified polyester fiber and 30-50 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of the polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:3.5-5:3-6.

[0007] Preferably, the preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol, and a silane coupling agent are added to anhydrous ethanol, stirred and ultrasonically treated for 5-10 hours to obtain a mixed dispersion; the mixed dispersion is then placed in a rotary evaporator for reduced pressure concentration to remove ethanol, thereby obtaining a carbon quantum dot / nanosilver / porous silica microsphere composite material.

[0008] The method for preparing the carbon quantum dots / nanosilver / porous silica microsphere composite material is simple and easy to operate. The carbon quantum dots / nanosilver / porous silica microsphere composite material prepared by the method can make the carbon quantum dots and nanosilver well dispersed in the modified polyester fiber.

[0009] Preferably, the mass ratio of the porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol, silane coupling agent, and anhydrous ethanol is 10: 0.05-0.1: 0.05-0.1: 0.03-0.06: 0.02-0.05: 70-100.

[0010] Preferably, the particle size range of the carbon quantum dots is 1-5 nm; the particle size range of the nanosilver is 1-50 nm; the polyethylene glycol is polyethylene glycol 800 or polyethylene glycol 1000; and the silane coupling agent is KH560 or KH570.

[0011] Preferably, the stirring speed is 100-150 r / min, and the power of the ultrasonic treatment is 200-350 W.

[0012] Preferably, the method for preparing the porous silica microspheres comprises the following steps: A template agent composed of sodium dodecylbenzene sulfonate and tetradecyltrimethylammonium bromide in a mass ratio of 2-3:1 is added to deionized water, and the mixture is stirred for 30-60 minutes to obtain a mixed solution; ethanol is then added to the mixed solution, and ammonia water is added after stirring, and tetraethyl orthosilicate is added dropwise after stirring for 2.5-3.5 hours. After the addition is completed, stirring is continued for 7-10 hours, and the mixture is allowed to stand for 5-10 hours, and then filtered, washed with ethanol and water, and then dried. The obtained product is placed in a muffle furnace for roasting at a temperature of 560-600°C and a roasting time of 5.5-7 hours to obtain the porous silica microspheres.

[0013] Preferably, the mass volume ratio of the deionized water, template, ethanol, ammonia water and tetraethyl orthosilicate is 1L:4.5-6g:0.4-0.6L:0.2-0.25L:26-32g; the mass fraction of the ammonia water is 25-28%.

[0014] The porous silica microspheres prepared by the method of the present invention have a large pore volume and specific surface area, and can better load carbon quantum dots and nanosilver.

[0015] Preferably, the method for preparing the modified polyester fiber comprises the following steps: Polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun to obtain modified polyester fibers.

[0016] Preferably, the melt spinning temperature is 260-290° C., and the spinning speed is 1000-2000 m / min.

[0017] As a general inventive concept, the present invention provides a method for preparing an antibacterial and mite-removing polyester blended wool fabric, comprising the following steps: S1, preparing wool into wool strips; preparing modified polyester fiber into polyester fiber strips; and drawing the wool strips and polyester fiber strips to obtain wool / polyester fiber mixed strips; S2, subjecting the wool / polyester fiber blended strip to roving, spun yarn, winding, doubling, and twisting in sequence to obtain a wool / polyester blended yarn; S3, weaving, dyeing and finishing the wool / polyester blended yarn to prepare the antibacterial and mite-removing polyester blended wool fabric.

[0018] The beneficial effects of the present invention are: The polyester blended wool fabric of the present invention adopts modified polyester fiber as antibacterial and mite-removing fiber. When preparing the modified polyester fiber, porous silica microspheres are used as carriers to load carbon quantum dots and nanosilver. The porous silica microspheres of the present invention have large pore volume and high specific surface area, and can absorb and accommodate more carbon quantum dots and nanosilver. In combination with adding an appropriate amount of polyethylene glycol and silane coupling agent, the porous silica microspheres are stably loaded with more carbon quantum dots and nanosilver, so that the carbon quantum dots and nanosilver are better dispersed in the polyester fiber, and their antibacterial and mite-removing properties are effectively exerted. In the carbon quantum dot / nanosilver / porous silica microsphere composite material of the present invention, on the basis of the excellent antibacterial and anti-mite and mite-removing properties of nanosilver, higher antibacterial properties can be obtained by combining carbon quantum dots with nanosilver, and it can be seen that carbon quantum dots and nanosilver have a certain synergistic effect.

[0019] At the same time, when preparing the carbon quantum dot / nanosilver / porous silica microsphere composite material, the compatibility between the composite material and polyester can be improved by adding polyethylene glycol and a silane coupling agent for modification, and when preparing the modified polyester fiber, an appropriate amount of ethylene-acrylate-maleic anhydride terpolymer is added to strengthen the bonding force between the porous silica microspheres and the polyester, thereby increasing the amount of the carbon quantum dot / nanosilver / porous silica microsphere composite material added to the polyester fiber, and making the modified polyester fiber have a higher strength, thereby effectively ensuring the product quality of the obtained polyester blended wool fabric and making it have a longer service life.

[0020] The polyester blended wool fabric of the invention has excellent antibacterial and anti-mite and mite removal performances, and the polyester fiber used has high strength, which can effectively ensure the product quality of the obtained polyester blended wool fabric and has strong durability. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Preparation Example 1: Add 6 g of template agent to 1 L of deionized water, the template agent is composed of sodium dodecylbenzene sulfonate and tetradecyltrimethylammonium bromide in a mass ratio of 2:1, and stir for 50 minutes to obtain a mixed solution; then add 0.4 L of ethanol to the mixed solution, stir and mix, then add 0.2 L of 25% ammonia water by mass, stir and add 30 g of ethyl orthosilicate dropwise for 3 hours, continue stirring for 10 hours after the addition is complete, let stand for 7 hours, then filter, wash with ethanol and water, and then dry, place the obtained product in a muffle furnace for roasting, the roasting temperature is 600°C, and the roasting time is 5.5 hours, so as to obtain porous silica microspheres.

[0023] Preparation Example 2: Add 4.5g of template agent to 1L of deionized water, the template agent is composed of sodium dodecylbenzene sulfonate and tetradecyltrimethylammonium bromide in a mass ratio of 3:1, stir for 60min to obtain a mixed solution; then add 0.6L of ethanol to the mixed solution, stir and mix, then add 0.25L of 25% ammonia water by mass, stir and add 32g of ethyl orthosilicate dropwise for 2.5h, continue stirring for 8h after the addition is complete, let stand for 10h, then filter, wash with ethanol and water, and then dry, place the obtained product in a muffle furnace for roasting, the roasting temperature is 580℃, and the roasting time is 6h to obtain porous silica microspheres.

[0024] Preparation Example 3: Add 5 g of template agent to 1 L of deionized water, the template agent is composed of sodium dodecylbenzenesulfonate and tetradecyltrimethylammonium bromide in a mass ratio of 3:1, and stir for 30 minutes to obtain a mixed solution; then add 0.6 L of ethanol to the mixed solution, stir and mix, then add 0.25 L of 25% ammonia water by mass, stir and add 26 g of tetraethyl orthosilicate dropwise for 3.5 hours, continue stirring for 7 hours after the addition is complete, let stand for 5 hours, then filter, wash with ethanol and water, and then dry, place the obtained product in a muffle furnace for roasting, the roasting temperature is 560°C, and the roasting time is 7 hours to obtain porous silica microspheres.

[0025] Embodiment 1: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 55 parts of modified polyester fiber and 45 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:4.5:4.

[0026] The preparation method of the modified polyester fiber comprises the following steps: The polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun at a melt spinning temperature of 270°C and a spinning speed of 1000m / min to obtain modified polyester fibers.

[0027] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 1), carbon quantum dots, nanosilver, polyethylene glycol 800, and silane coupling agent KH560 are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 150r / min, and the power of ultrasonic treatment is 200W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0028] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol 800, silane coupling agent KH560, and anhydrous ethanol is 10: 0.05: 0.08: 0.03: 0.04: 80. The particle size of carbon quantum dots is in the range of 1-5nm; the particle size of nanosilver is in the range of 1-50nm.

[0029] The method for preparing the antibacterial and mite-removing polyester blended wool fabric in this embodiment comprises the following steps: S1, preparing wool into wool strips; preparing modified polyester fiber into polyester fiber strips; and drawing the wool strips and polyester fiber strips to obtain wool / polyester fiber mixed strips; S2, subjecting the wool / polyester fiber blended strip to roving, spun yarn, winding, doubling, and twisting in sequence to obtain a wool / polyester blended yarn; S3, weaving, dyeing and finishing the wool / polyester blended yarn to prepare the antibacterial and mite-removing polyester blended wool fabric.

[0030] Embodiment 2: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 50 parts of modified polyester fiber and 50 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:4:6.

[0031] The preparation method of the modified polyester fiber comprises the following steps: The polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun at a melt spinning temperature of 280°C and a spinning speed of 1500m / min to obtain modified polyester fibers.

[0032] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 3), carbon quantum dots, nanosilver, polyethylene glycol 1000, and silane coupling agent KH570 are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 120r / min, and the power of ultrasonic treatment is 300W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0033] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol 1000, silane coupling agent KH570, and anhydrous ethanol is 10: 0.09: 0.05: 0.05: 0.02: 100. The particle size of carbon quantum dots ranges from 1 to 5 nm; the particle size of nanosilver ranges from 1 to 50 nm.

[0034] The preparation method of the antibacterial and mite-removing polyester blended wool fabric in this embodiment is the same as that in Example 1.

[0035] Embodiment 3: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 60 parts of modified polyester fiber and 40 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:4.5:3.

[0036] The preparation method of the modified polyester fiber comprises the following steps: The polyester, carbon quantum dot / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun at a melt spinning temperature of 290°C and a spinning speed of 2000m / min to obtain modified polyester fibers.

[0037] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 1), carbon quantum dots, nanosilver, polyethylene glycol 1000, and silane coupling agent KH570 are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 150r / min, and the power of ultrasonic treatment is 300W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0038] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol 1000, silane coupling agent KH570, and anhydrous ethanol is 10: 0.1: 0.07: 0.03: 0.02: 80. The particle size of carbon quantum dots is in the range of 1-5 nm; the particle size of nanosilver is in the range of 1-50 nm.

[0039] The preparation method of the antibacterial and mite-removing polyester blended wool fabric in this embodiment is the same as that in Example 1.

[0040] Embodiment 4: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 70 parts of modified polyester fiber and 30 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:5:6.

[0041] The preparation method of the modified polyester fiber comprises the following steps: The polyester, carbon quantum dot / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun at a melt spinning temperature of 260°C and a spinning speed of 1500m / min to obtain modified polyester fibers.

[0042] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 1), carbon quantum dots, nanosilver, polyethylene glycol 800, and silane coupling agent KH560 are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 120r / min, the power of ultrasonic treatment is 350W, and a mixed dispersion is obtained; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0043] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol 800, silane coupling agent KH560, and anhydrous ethanol is 10: 0.05: 0.1: 0.05: 0.02: 90. The particle size of carbon quantum dots is in the range of 1-5 nm; the particle size of nanosilver is in the range of 1-50 nm.

[0044] The preparation method of the antibacterial and mite-removing polyester blended wool fabric in this embodiment is the same as that in Example 1.

[0045] Embodiment 5: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 65 parts of modified polyester fiber and 35 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:3.5:4.5.

[0046] The preparation method of the modified polyester fiber comprises the following steps: The polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun at a melt spinning temperature of 290°C and a spinning speed of 1000m / min to obtain modified polyester fibers.

[0047] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 3), carbon quantum dots, nanosilver, polyethylene glycol 800, and silane coupling agent KH570 are added to anhydrous ethanol, stirred and ultrasonically treated for 5 hours, the stirring speed is 100 r / min, and the power of the ultrasonic treatment is 200 W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0048] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol 800, silane coupling agent KH570, and anhydrous ethanol is 10: 0.1: 0.05: 0.03: 0.05: 100. The particle size of carbon quantum dots is in the range of 1-5 nm; the particle size of nanosilver is in the range of 1-50 nm.

[0049] The preparation method of the antibacterial and mite-removing polyester blended wool fabric in this embodiment is the same as that in Example 1.

[0050] Embodiment 6: An antibacterial and mite-removing polyester blended wool fabric comprises the following raw materials in parts by weight: 55 parts of modified polyester fiber and 45 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:4:4.5.

[0051] The preparation method of the modified polyester fiber comprises the following steps: The polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun at a melt spinning temperature of 270°C and a spinning speed of 1000m / min to obtain modified polyester fibers.

[0052] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 2), carbon quantum dots, nanosilver, polyethylene glycol 1000, and silane coupling agent KH560 are added to anhydrous ethanol, stirred and ultrasonically treated for 7 hours, the stirring speed is 150r / min, the power of the ultrasonic treatment is 300W, and a mixed dispersion is obtained; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0053] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol 1000, silane coupling agent KH560, and anhydrous ethanol is 10: 0.07: 0.07: 0.06: 0.03: 70. The particle size of carbon quantum dots is in the range of 1-5 nm; the particle size of nanosilver is in the range of 1-50 nm.

[0054] The preparation method of the antibacterial and mite-removing polyester blended wool fabric in this embodiment is the same as that in Example 1.

[0055] Comparative Example 1: Different from the embodiment, the raw materials of the modified polyester fiber include polyester, nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:4.5:4.

[0056] The preparation method of the nano silver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 1), nanosilver, polyethylene glycol 800, and silane coupling agent KH560 are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 150r / min, and the power of ultrasonic treatment is 200W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0057] The mass ratio of porous silica microspheres, nanosilver, polyethylene glycol 800, silane coupling agent KH560, and anhydrous ethanol is 10: 0.13: 0.03: 0.04: 80. The particle size of the nanosilver is in the range of 1-50 nm.

[0058] Comparative Example 2: Different from the embodiment, the raw materials of the modified polyester fiber include polyester, carbon quantum dots / porous silica microspheres composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of polyester, carbon quantum dots / porous silica microspheres composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:4.5:4.

[0059] The preparation method of the carbon quantum dot / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 1), carbon quantum dots, polyethylene glycol 800, and silane coupling agent KH560 are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 150r / min, and the power of ultrasonic treatment is 200W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0060] The mass ratio of porous silica microspheres, carbon quantum dots, polyethylene glycol 800, silane coupling agent KH560, and anhydrous ethanol is 10: 0.13: 0.03: 0.04: 80. The particle size of the carbon quantum dots ranges from 1 to 5 nm.

[0061] Comparative Example 3: Different from the embodiment, the raw materials of the modified polyester fiber include polyester and carbon quantum dots / nanosilver / porous silica microsphere composite materials; the mass ratio of the polyester and carbon quantum dots / nanosilver / porous silica microsphere composite materials is 100:4.5.

[0062] The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres (prepared by the method in Preparation Example 1), carbon quantum dots, and nanosilver are added to anhydrous ethanol, stirred and ultrasonically treated for 10 hours, the stirring speed is 150r / min, and the power of ultrasonic treatment is 200W to obtain a mixed dispersion; then the mixed dispersion is placed in a rotary evaporator for reduced pressure concentration to remove ethanol, and a carbon quantum dot / nanosilver / porous silica microsphere composite material is obtained.

[0063] The mass ratio of porous silica microspheres, carbon quantum dots, nanosilver and anhydrous ethanol is 10: 0.05: 0.08: 80. The particle size of the carbon quantum dots is in the range of 1-5 nm; the particle size of the nanosilver is in the range of 1-50 nm.

[0064] Performance Testing 1. Referring to GB / T 20944.3-2009 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the antibacterial properties of polyester blended wool fabrics in Examples 1-6 and Comparative Examples 1-3 were tested, and the antibacterial and anti-mite properties of antibacterial and anti-mite polyester blended wool fabrics in Examples 1-6 and Comparative Examples 1-3 were tested according to GBT24253-2009 "Evaluation of anti-mite properties of textiles", and the repellency rate and inhibition rate of polyester blended wool fabrics to mites were calculated. The test results are shown in Table 1.

[0065] Table 1:

[0066] As shown in Table 1, the polyester blended wool fabrics prepared in Examples 1-6 of the present invention have excellent antibacterial and anti-mite properties. By comparing Example 1 with Comparative Examples 1-2, it can be seen that the antibacterial and anti-mite properties of the obtained polyester blended wool fabrics are significantly better than those of the nanosilver / porous silica microsphere composites and the carbon quantum dots / porous silica microsphere composites. By comparing Example 1 with Comparative Example 3, it can be seen that when preparing the carbon quantum dots / nanosilver / porous silica microsphere composites, polyethylene glycol and silane coupling agents are added for modification, and when preparing the modified polyester fiber, an appropriate amount of ethylene-acrylate-maleic anhydride terpolymer is added, which can also slightly enhance the antibacterial and anti-mite properties of the polyester blended wool fabrics. It may be that through the above operation, the dispersibility of the carbon quantum dots / nanosilver / porous silica microsphere composites in the fibers can be increased, and the dispersion in the fibers is more uniform, thereby better exerting the antibacterial and anti-mite properties.

[0067] 2. The breaking strength of the modified polyester fibers prepared in Examples 1-6 and Comparative Examples 1-3 was tested. In addition, polyester fibers were prepared using only polyester as raw material, and their breaking strength was tested, and the polyester fibers were used as a control group. The preparation method of the polyester fibers was as follows: polyester was placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain polyester pellets; the polyester pellets were melt-spun at a temperature of 270°C and a spinning speed of 1000 m / min to obtain polyester fibers. The specific test results of the breaking strength are shown in Table 2.

[0068] Table 2:

[0069] As shown in Table 2, the modified polyester fibers prepared by the methods of Examples 1-6 of the present invention still have a relatively high breaking strength, and thus can maintain excellent spinnability, so that the prepared polyester blended wool fabric has a relatively high product quality and strong durability. As shown in Comparative Example 3 and Example 1, if no polyethylene glycol or silane coupling agent is added for modification when preparing the carbon quantum dot / nanosilver / porous silica microsphere composite material, and no ethylene-acrylate-maleic anhydride terpolymer is added when preparing the modified polyester fiber, the strength of the obtained modified polyester fiber will be significantly reduced.

[0070] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An antibacterial and mite-removing polyester blended wool fabric, characterized in that: The method comprises the following raw materials in parts by weight: 50-70 parts of modified polyester fiber and 30-50 parts of wool; The raw materials of the modified polyester fiber include polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer; the mass ratio of the polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material, and ethylene-acrylate-maleic anhydride terpolymer is 100:3.5-5:3-6.

2. The antibacterial and mite-removing polyester blended wool fabric according to claim 1, characterized in that: The preparation method of the carbon quantum dot / nanosilver / porous silica microsphere composite material comprises the following steps: Porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol, and a silane coupling agent are added to anhydrous ethanol, stirred and ultrasonically treated for 5-10 hours to obtain a mixed dispersion; the mixed dispersion is then placed in a rotary evaporator for reduced pressure concentration to remove ethanol, thereby obtaining a carbon quantum dot / nanosilver / porous silica microsphere composite material.

3. The antibacterial and mite-removing polyester blended wool fabric according to claim 2, characterized in that: The mass ratio of the porous silica microspheres, carbon quantum dots, nanosilver, polyethylene glycol, silane coupling agent and anhydrous ethanol is 10: 0.05-0.1: 0.05-0.1: 0.03-0.06: 0.02-0.05: 70-100.

4. The antibacterial and mite-removing polyester blended wool fabric according to claim 2, characterized in that: The particle size range of the carbon quantum dots is 1-5 nm; the particle size range of the nanosilver is 1-50 nm; the polyethylene glycol is polyethylene glycol 800 or polyethylene glycol 1000; and the silane coupling agent is KH560 or KH570.

5. The antibacterial and mite-removing polyester blended wool fabric as claimed in claim 2, wherein the stirring speed is 100-150 r / min, and the power of the ultrasonic treatment is 200-350 W.

6. The antibacterial and mite-removing polyester blended wool fabric according to claim 1, characterized in that: The method for preparing the porous silica microspheres comprises the following steps: A template agent composed of sodium dodecylbenzene sulfonate and tetradecyltrimethylammonium bromide in a mass ratio of 2-3:1 is added to deionized water, and the mixture is stirred for 30-60 minutes to obtain a mixed solution; ethanol is then added to the mixed solution, and ammonia water is added after stirring, and tetraethyl orthosilicate is added dropwise after stirring for 2.5-3.5 hours. After the addition is completed, stirring is continued for 7-10 hours, and the mixture is allowed to stand for 5-10 hours, and then filtered, washed with ethanol and water, and then dried. The obtained product is placed in a muffle furnace for roasting at a temperature of 560-600°C and a roasting time of 5.5-7 hours to obtain the porous silica microspheres.

7. The antibacterial and mite-removing polyester blended wool fabric according to claim 6, characterized in that: The mass volume ratio of the deionized water, template, ethanol, ammonia water and tetraethyl orthosilicate is 1L: 4.5-6g: 0.4-0.6L: 0.2-0.25L: 26-32g; the mass fraction of the ammonia water is 25-28%.

8. The antibacterial and mite-removing polyester blended wool fabric according to claim 1, characterized in that: The preparation method of the modified polyester fiber comprises the following steps: Polyester, carbon quantum dots / nanosilver / porous silica microsphere composite material and ethylene-acrylate-maleic anhydride terpolymer are mixed evenly, and then placed in a twin-screw extruder for blending, melt extrusion and granulation to obtain modified polyester pellets; the modified polyester pellets are melt-spun to obtain modified polyester fibers.

9. The antibacterial and mite-removing polyester blended wool fabric according to claim 8, characterized in that: The temperature of the melt spinning is 260-290° C., and the spinning speed is 1000-2000 m / min.

10. A method for preparing the antibacterial and mite-removing polyester blended wool fabric according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, preparing wool into wool strips; preparing modified polyester fiber into polyester fiber strips; and drawing the wool strips and polyester fiber strips to obtain wool / polyester fiber mixed strips; S2, subjecting the wool / polyester fiber blended strip to roving, spun yarn, winding, doubling, and twisting in sequence to obtain a wool / polyester blended yarn; S3, weaving, dyeing and finishing the wool / polyester blended yarn to prepare the antibacterial and mite-removing polyester blended wool fabric.

Citation Information

Patent Citations

  • Toughened halogen-free flame-retardant polylactic acid blending material

    CN101831156A

  • Functional polyester fiber and its manufacture method

    CN102345184A

  • Method for preparing medicine-carrying nanofibers of core-shell structure by virtue of Pickering emulsion electrospinning

    CN104947229A

  • Antibacterial master batch, polyester DTY (Draw Textured Yarn) using antibacterial master batch and production method of polyester DTY

    CN113913000A

  • Wool and coffee carbon modified polyester blended yarn and fabric production method

    CN113913983A

Cited By

  • Antibacterial flexible silica gel rubber compound and preparation method thereof

    CN120648235A