Durable antistatic polyester textile
By using antistatic agents and blending technology of polyester fibers and metal fibers in polyester textiles, a conductive network is formed, which solves the static problem of polyester textiles, significantly improves antistatic durability and wear comfort, and reduces dust absorption and skin irritation. risk.
Patent Information
- Application Number
- CN202411011941.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing polyester textiles on the market have poor anti-static effect and are prone to static electricity, which leads to entanglement and adsorbing dust in clothing, affecting the comfort of wearing.
Antistatic agents are used to mix and stir with polyester fibers, and spin them through a spinning machine. The metal fibers are blended with spinning to form a conductive network to reduce electrostatic adsorption.
It effectively improves the anti-static durability of polyester textiles, prevents electrostatic entanglement, maintains comfortable wearing, and reduces dust absorption, protects skin health.
Smart Images

Figure HDA0004964636060000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile processing, and in particular relates to a durable antistatic polyester textile. Background Art
[0002] Polyester textiles are a type of widely used textiles. Polyester, also known as polyester fiber, is a synthetic fiber with excellent wrinkle resistance, shape retention and abrasion resistance. It also has high strength and elastic recovery. Therefore, polyester textiles have a wide range of applications, including clothing, home textiles, industrial fabrics, etc. Wrinkle resistance: Polyester fabrics are not easy to wrinkle, easy to care for and keep their shape. The wear resistance of polyester far exceeds that of natural fibers and general chemical fibers, and is suitable for making products that require high wear resistance. Polyester fabrics have good elastic recovery ability, are comfortable to wear and not easy to deform. Polyester has good resistance to chemicals such as acids and alkalis, and is not easily corroded. Polyester textiles are easy to wash and dry, and are suitable for a fast-paced lifestyle;
[0003] However, the existing polyester textiles on the market have poor antistatic effects. After the textiles are used and rubbed, a large amount of static electricity is generated, which easily absorbs dust and flying hair. When wearing polyester clothes, due to the effect of static electricity, the clothes are easily entangled, such as "skirt hugging the legs", etc., which brings inconvenience to the wearer. In this regard, we have proposed a durable antistatic polyester textile. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides a durable antistatic polyester textile to solve the above technical problems.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a durable antistatic polyester textile, which is prepared from the following materials: 100-600 parts of terephthalic acid, 100-500 parts of ethylene glycol, 120-980 parts of cotton, 320-1300 parts of hemp, 100-630 parts of metal fiber and 10-320 parts of antistatic agent.
[0006] Preferably, the polyester textile is made of the following materials: 270 parts of terephthalic acid, 230 parts of ethylene glycol, 880 parts of cotton, 1100 parts of linen, 320 parts of metal fiber and 120 parts of antistatic agent.
[0007] Preferably, terephthalic acid and ethylene glycol are polymerized to generate polyester fibers, and the carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo an esterification reaction in the presence of a catalyst to generate an ester bond and water, and the reaction formula is:
[0008] nHOOC-C6H4-COOH+nHO-2CH2-OH→nOOC-C6H4-COO-2CH2-O+2nH2OAs the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain. During the reaction, water molecules are discharged from the reaction system to promote the reverse generation of polymer products and convert them into polyethylene terephthalate. After the reaction is completed, the polyethylene terephthalate is subjected to a condensation reaction at a temperature of 250°C-300°C and a vacuum environment to remove small molecules and form a polyester melt; the product is solidified and cooled to stabilize the structure, and is pelletized to obtain polyester fiber particles.
[0009] Preferably, the cotton is one of knitted cotton, washed cotton, organic cotton and mercerized cotton, the hemp is one of hemp, flax, ramie, jute, sisal and abaca, and the metal fiber is carbon fiber.
[0010] Preferably, the preparation step of the antistatic agent comprises preparing the following materials: acrylic acid, 2-hydroxyethyl methacrylate, ethyl methacrylate, butyl acrylate, octadecyl acrylate and ethyl acrylate; stirring and mixing the prepared materials in proportion, adding isopropanol to the mixed materials, carrying out polymerization reaction at a temperature of 80° C.-85° C. in the presence of azobisisobutyronitrile for 6 hours, and uniformly mixing the product after the polymerization reaction with triethylamine, water and polyhydroxy glycidyl ether to obtain the antistatic agent.
[0011] Preferably, the preparation step of the metal fiber is to prepare polyacrylonitrile material, soak the polyacrylonitrile in deionized water for 2 hours, remove impurities, dissolve the dried polyacrylonitrile in a solvent to prepare a spinning solution, spin the spinning solution into fibers through a spinning machine, place the formed fibers in an oxidation furnace for oxidation treatment, and then undergo high-temperature carbonization treatment to become pure carbon fibers.
[0012] Preferably, the textile antistatic treatment step is:
[0013] A1. Mixing and stirring the antistatic agent with the polyester fiber prepared from terephthalic acid and ethylene glycol;
[0014] A2. After the stirring is completed, the material is placed in a spinning machine for spinning;
[0015] A3. Weaving the spun silk threads, blending the metal fibers with the spun silk threads, and weaving the metal fibers into the fabric to form a conductive network.
[0016] Preferably, the blending and weaving steps in step A3 are performed by stretching and cutting the metal fibers in filament bundles to make short fiber strips with the same length as the spinning material, controlling the length and fineness of the fibers, mixing the treated metal short fibers with the spinning material, mixing the metal fiber particles into the spinning solution, and spinning the evenly mixed spinning solution through a spinning machine to form composite fibers containing metal fibers.
[0017] Preferably, the ratio of terephthalic acid to ethylene glycol is 2.7:2.3.
[0018] Preferably, the prepared textile is tested for antistatic properties.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present application uses an antistatic agent to mix and stir polyester fibers, weaves the spun silk threads, blends the metal fibers with the spun threads, and weaves the metal fibers into the fabric to form a conductive network. This can effectively make the prepared polyester textiles anti-static, prevent the adsorption and entanglement phenomenon caused by static electricity on the fabric, and improve the anti-static durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The figure is a flowchart of the steps of antistatic treatment of textiles according to the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The invention provides a technical solution: a durable antistatic polyester textile, which is prepared from the following materials: 100-600 parts of terephthalic acid, 100-500 parts of ethylene glycol, 120-980 parts of cotton, 320-1300 parts of hemp, 100-630 parts of metal fiber and 10-320 parts of antistatic agent.
[0024] Furthermore, the polyester textile is specifically prepared from the following materials: 270 parts of terephthalic acid, 230 parts of ethylene glycol, 880 parts of cotton, 1100 parts of hemp, 320 parts of metal fiber and 120 parts of antistatic agent;
[0025] Antistatic agent is a chemical substance that can reduce the surface resistance of materials and increase electrical conductivity. When antistatic agent is added to polymer materials, it can form a conductive layer on the surface of the material, allowing static charge to be released quickly, thereby achieving an antistatic effect.
[0026] Further, terephthalic acid and ethylene glycol undergo a polymerization reaction to generate polyester fibers. The carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo an esterification reaction in the presence of a catalyst to generate an ester bond and water. The reaction formula is:
[0027] nHOOC-C6H4-COOH+nHO-2CH2-OH→nOOC-C6H4-COO-2CH2-O+2nH2OAs the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain. During the reaction, water molecules are discharged from the reaction system to promote the reverse generation of polymer products and convert them into polyethylene terephthalate. After the reaction is completed, the polyethylene terephthalate is subjected to a condensation reaction at a temperature of 250°C-300°C and a vacuum environment to remove small molecules and form a polyester melt; the product is solidified and cooled to stabilize the structure, and is pelletized to obtain polyester fiber particles.
[0028] Furthermore, the cotton is one of knitted cotton, washed cotton, organic cotton and mercerized cotton, the hemp is one of hemp, flax, ramie, jute, sisal and abaca, and the metal fiber is carbon fiber.
[0029] Furthermore, the preparation step of the antistatic agent includes preparing the following materials: acrylic acid, 2-hydroxyethyl methacrylate, ethyl methacrylate, butyl acrylate, octadecyl acrylate and ethyl acrylate; stirring and mixing the prepared materials in proportion, adding isopropanol to the mixed materials, and performing a polymerization reaction at a temperature of 80°C-85°C in the presence of azobisisobutyronitrile for 6 hours, and uniformly mixing the product after the polymerization reaction with triethylamine, water and polyhydroxy glycidyl ether to obtain an antistatic agent.
[0030] Furthermore, the preparation step of the metal fiber includes preparing polyacrylonitrile material, soaking the polyacrylonitrile in deionized water for 2 hours, removing impurities, dissolving the dried polyacrylonitrile in a solvent to prepare a spinning solution, spinning the spinning solution into fibers through a spinning machine, placing the formed fibers in an oxidation furnace for oxidation treatment, and then undergoing high-temperature carbonization treatment to become pure carbon fibers;
[0031] The preparation process of metal fiber involves multiple links such as raw material selection and preparation, spinning molding, pre-oxidation treatment, carbonization treatment, surface treatment and sizing, subsequent processing and product preparation. Each link requires strict control of process parameters and equipment conditions to ensure the performance and quality of the final product.
[0032] Further, the steps of antistatic treatment of textiles are:
[0033] A1. Mixing and stirring the antistatic agent with the polyester fiber prepared from terephthalic acid and ethylene glycol;
[0034] A2. After the stirring is completed, the material is placed in a spinning machine for spinning;
[0035] A3, weaving the spun silk threads, blending the metal fibers with the spun silk threads, and weaving the metal fibers into the fabric to form a conductive network;
[0036] The antistatic treatment step is simple to operate, low in cost, applicable to a variety of polymer materials, has a lasting antistatic effect, and does not affect the air permeability and feel of the fabric.
[0037] Furthermore, the blending and weaving step in step A3 is carried out by stretching and cutting the filament bundle-shaped metal fibers to make short fiber strips with the same length as the spinning material, controlling the length and fineness of the fibers, mixing the processed metal short fibers with the spinning material, mixing the metal fiber particles into the spinning solution, and spinning the evenly mixed spinning solution through a spinning machine to form a composite fiber containing metal fibers.
[0038] Furthermore, the ratio of terephthalic acid to ethylene glycol is 2.7:2.3.
[0039] Furthermore, the antistatic properties of the prepared textiles were tested.
[0040] Example 1
[0041] The preparation steps of a durable antistatic polyester textile are as follows:
[0042] S1. Prepare the following materials: 270 parts of terephthalic acid, 230 parts of ethylene glycol, 880 parts of cotton, 1100 parts of hemp, 320 parts of metal fiber and 120 parts of antistatic agent;
[0043] S2, preparing polyester fiber, the carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo esterification reaction in the presence of a catalyst to generate ester bonds and water, as the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain, during the reaction, water molecules are discharged from the reaction system, driving the reverse generation of polymer products, and converting into polyethylene terephthalate, after the reaction is completed, the polyethylene terephthalate is subjected to a condensation reaction at a temperature of 250° C. to 300° C. and a vacuum environment to remove small molecules to form a polyester melt, the product is solidified and cooled to stabilize the structure, and pelletized to obtain polyester fiber particles;
[0044] S3, antistatic treatment, mixing the antistatic agent, polyester fiber, cotton and linen, after the mixing is completed, putting the materials into a spinning machine for spinning treatment, weaving the spun silk thread, blending the metal fiber with the spun silk, weaving the metal fiber into the fabric to form a conductive network;
[0045] S4: Cut, inspect and store the prepared fabrics.
[0046] Example 2
[0047] The preparation steps of a durable antistatic polyester textile are as follows:
[0048] S1. Prepare the following materials: 500 parts of terephthalic acid, 230 parts of ethylene glycol, 560 parts of cotton, 1200 parts of hemp, 220 parts of metal fiber and 100 parts of antistatic agent;
[0049] S2, preparing polyester fiber, the carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo esterification reaction in the presence of a catalyst to generate ester bonds and water, as the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain, during the reaction, water molecules are discharged from the reaction system, driving the reverse generation of polymer products, and converting into polyethylene terephthalate, after the reaction is completed, the polyethylene terephthalate is subjected to condensation reaction at a temperature of 270°C-300°C and a vacuum environment to remove small molecules to form a polyester melt, the product is solidified and cooled to stabilize the structure, and pelletized to obtain polyester fiber particles;
[0050] S3, antistatic treatment, mixing the antistatic agent, polyester fiber, cotton and linen, after the mixing is completed, putting the materials into a spinning machine for spinning treatment, weaving the spun silk thread, blending the metal fiber with the spun silk, weaving the metal fiber into the fabric to form a conductive network;
[0051] S4: Cut, inspect and store the prepared fabrics.
[0052] Example 3
[0053] The preparation steps of a durable antistatic polyester textile are as follows:
[0054] S1. Prepare the following materials: 560 parts of terephthalic acid, 410 parts of ethylene glycol, 560 parts of cotton, 1300 parts of hemp, 260 parts of metal fiber and 250 parts of antistatic agent;
[0055] S2, preparing polyester fiber, the carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo esterification reaction in the presence of a catalyst to generate ester bonds and water, as the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain, during the reaction, water molecules are discharged from the reaction system, driving the reverse generation of polymer products, and converting into polyethylene terephthalate, after the reaction is completed, the polyethylene terephthalate is subjected to condensation reaction at a temperature of 230°C-300°C and a vacuum environment to remove small molecules to form a polyester melt, the product is solidified and cooled to stabilize the structure, and pelletized to obtain polyester fiber particles;
[0056] S3, antistatic treatment, mixing the antistatic agent, polyester fiber, cotton and linen, after the mixing is completed, putting the materials into a spinning machine for spinning treatment, weaving the spun silk thread, blending the metal fiber with the spun silk, weaving the metal fiber into the fabric to form a conductive network;
[0057] S4: Cut, inspect and store the prepared fabrics.
[0058] Example 4
[0059] The preparation steps of a durable antistatic polyester textile are as follows:
[0060] S1. Prepare the following materials: 320 parts of terephthalic acid, 450 parts of ethylene glycol, 900 parts of cotton, 1200 parts of hemp, 330 parts of metal fiber and 110 parts of antistatic agent;
[0061] S2, preparing polyester fiber, the carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo esterification reaction in the presence of a catalyst to generate ester bonds and water, as the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain, during the reaction, water molecules are discharged from the reaction system, driving the reverse generation of polymer products, and converting into polyethylene terephthalate, after the reaction is completed, the polyethylene terephthalate is subjected to a condensation reaction at a temperature of 250° C. to 300° C. and a vacuum environment to remove small molecules to form a polyester melt, the product is solidified and cooled to stabilize the structure, and pelletized to obtain polyester fiber particles;
[0062] S3, antistatic treatment, mixing the antistatic agent, polyester fiber, cotton and linen, after the mixing is completed, putting the materials into a spinning machine for spinning treatment, weaving the spun silk thread, blending the metal fiber with the spun silk, weaving the metal fiber into the fabric to form a conductive network;
[0063] S4: Cut, inspect and store the prepared fabrics.
[0064] Comparative Example 1
[0065] The preparation steps of polyester textiles are:
[0066] S1. Prepare the following materials: 270 parts of terephthalic acid, 230 parts of ethylene glycol, 880 parts of cotton and 1100 parts of hemp;
[0067] S2, preparing polyester fiber, the carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo esterification reaction in the presence of a catalyst to generate ester bonds and water, as the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain, during the reaction, water molecules are discharged from the reaction system, driving the reverse generation of polymer products, and converting into polyethylene terephthalate, after the reaction is completed, the polyethylene terephthalate is subjected to a condensation reaction at a temperature of 250° C. to 300° C. and a vacuum environment to remove small molecules to form a polyester melt, the product is solidified and cooled to stabilize the structure, and pelletized to obtain polyester fiber particles;
[0068] S3, mixing the polyester fiber particles with cotton and linen, and sending the mixture into a spinning machine for spinning to produce fabrics;
[0069] S4: Cut, inspect and store the prepared fabrics.
[0070] Table 1 below shows the antistatic properties of textiles prepared in different embodiments and comparative examples.
[0071] Group Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Antistatic Excellent Excellent Excellent Excellent ordinary
[0072] Table 1
[0073] Antistatic Testing Steps
[0074] Prepare samples for polyester textile testing, ensuring that the specimen size and tension meet the requirements;
[0075] Under a certain tension, rub the sample against the standard cloth until the sample is charged and reaches a stable state;
[0076] Use a voltmeter to measure the maximum voltage and average voltage of the sample;
[0077] The antistatic performance of the sample is determined based on the measured voltage value and the range required by the standard.
[0078] The textile in comparative example 1 has poor antistatic effect. After friction occurs during use, a large amount of static electricity is generated, which easily absorbs dust and flying hair. When wearing polyester clothing, due to the effect of static electricity, clothing is easily entangled, such as "skirt hugging legs", etc., which brings inconvenience to the wearer. The textile in the embodiment can effectively reduce or eliminate static electricity, avoid electric shock and discomfort caused by static electricity when wearing, especially in a dry environment. The antistatic function is particularly important and can significantly improve the comfort of wearing. Static electricity may have an irritating effect on human skin. Long-term contact with static electricity may also cause skin allergies, dermatitis and other problems. Antistatic polyester textiles can significantly reduce this risk and protect human skin health. At the same time, the antistatic function can also reduce the potential harm of static electricity to the human body, such as reducing blood sugar concentration fluctuations. Static electricity easily absorbs dust and flying hair in the air, causing pollution and damage to the surface of textiles. Antistatic polyester textiles can effectively reduce this adsorption phenomenon and keep the product clean and beautiful.
[0079] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A durable antistatic polyester textile, characterized in that: The polyester textile is prepared from the following materials: 100-600 parts of terephthalic acid, 100-500 parts of ethylene glycol, 120-980 parts of cotton, 320-1300 parts of hemp, 100-630 parts of metal fiber and 10-320 parts of antistatic agent.
2. The durable antistatic polyester textile according to claim 1, characterized in that: The polyester textile is specifically prepared from the following materials: 270 parts of terephthalic acid, 230 parts of ethylene glycol, 880 parts of cotton, 1100 parts of hemp, 320 parts of metal fiber and 120 parts of antistatic agent.
3. The durable antistatic polyester textile according to claim 1, characterized in that: Terephthalic acid and ethylene glycol undergo polymerization reaction to produce polyester fiber. The carboxyl group of terephthalic acid and the hydroxyl group of ethylene glycol undergo esterification reaction in the presence of a catalyst to produce an ester bond and water. The reaction formula is: nHOOC-C6H4-COOH+nHO-2CH2-OH→nOOC-C6H4-COO-2CH2-O+2nH2OAs the esterification reaction proceeds, the generated ester bonds increase to form a polymer chain. During the reaction, water molecules are discharged from the reaction system to promote the reverse generation of polymer products and convert them into polyethylene terephthalate. After the reaction is completed, the polyethylene terephthalate is subjected to a condensation reaction at a temperature of 250°C-300°C and a vacuum environment to remove small molecules and form a polyester melt; the product is solidified and cooled to stabilize the structure, and is pelletized to obtain polyester fiber particles.
4. The durable antistatic polyester textile according to claim 1, characterized in that: The cotton is one of knitted cotton, washed cotton, organic cotton and mercerized cotton, the hemp is one of hemp, flax, ramie, jute, sisal and abaca, and the metal fiber is carbon fiber.
5. The durable antistatic polyester textile according to claim 1, characterized in that: The preparation steps of the antistatic agent include preparing the following materials: acrylic acid, 2-hydroxyethyl methacrylate, ethyl methacrylate, butyl acrylate, octadecyl acrylate and ethyl acrylate; stirring and mixing the prepared materials according to a proportion, adding isopropanol to the mixed materials, and carrying out a polymerization reaction at a temperature of 80° C.-85° C. in the presence of azobisisobutyronitrile for 6 hours, and uniformly mixing the product after the polymerization reaction with triethylamine, water and polyhydroxy glycidyl ether to obtain the antistatic agent.
6. The durable antistatic polyester textile according to claim 1, characterized in that: The preparation steps of the metal fiber are as follows: prepare polyacrylonitrile material, soak the polyacrylonitrile in deionized water for 2 hours, remove impurities, dissolve the dried polyacrylonitrile in a solvent to make a spinning solution, spin the spinning solution into fibers through a spinning machine, place the formed fibers in an oxidation furnace for oxidation treatment, and then undergo high-temperature carbonization treatment to become pure carbon fibers.
7. The durable antistatic polyester textile according to claim 1, characterized in that: The steps for antistatic treatment of textiles are: A1. Mixing and stirring the antistatic agent with the polyester fiber prepared from terephthalic acid and ethylene glycol; A2. After the stirring is completed, the material is placed in a spinning machine for spinning; A3. Weaving the spun silk threads, blending the metal fibers with the spun silk threads, and weaving the metal fibers into the fabric to form a conductive network.
8. The durable antistatic polyester textile according to claim 7, characterized in that: The blending and weaving steps in step A3 are carried out by stretching and cutting the metal fibers in filament bundles to make short fiber strips with the same length as the spinning material, controlling the length and fineness of the fibers, mixing the processed metal short fibers with the spinning material, mixing the metal fiber particles into the spinning solution, and spinning the evenly mixed spinning solution through a spinning machine to form composite fibers containing metal fibers.
9. The durable antistatic polyester textile according to claim 2, characterized in that: The ratio of terephthalic acid to ethylene glycol is 2.7:2.
3.
10. The durable antistatic polyester textile according to claim 1, characterized in that: The antistatic properties of the prepared textiles were tested.
Citation Information
Patent Citations
Wear-resisting anti-crease cotton blended yarn
CN105386180A
Anti-static textile preparation method
CN111020797A
Anti-mildew carbon fiber polyester thread and production method thereof
CN114318606A
Antistatic polyurethane film and preparation method thereof
CN115431618A