Lens antifogging cloth and preparation method thereof
The lens anti-fog cloth treated with island fibers and nano-silver film solves the problem that traditional lens wipes cannot prevent mist formation for a long time, and achieves effective anti-fog and anti-bacterial functions, extends service life and improves the convenience of lens cleaning. and security.
Patent Information
- Application Number
- CN202410974459.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional lens wipes cannot effectively prevent mist formation for a long time, and the anti-fog effect gradually weakens after use, affecting life and personal safety.
The lens anti-fog cloth made of island fibers has a surfactant, anti-fog layer and anti-bacterial layer. By soaking the anti-fog agent and nano-silver film, it forms a serrated cloth surface, providing anti-fog and anti-bacterial functions.
Effectively remove mist and bacteria from the lens, extend service life, reduce repeated wipes, provide long-lasting anti-fog and antibacterial effects, and improve the convenience and safety of lens cleaning.
Smart Images

Figure CN118910889A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lens cleaning cloths, and in particular relates to an anti-fog cloth for lenses and a preparation method thereof. Background Art
[0002] With the increasing number of myopic people, the use rate of glasses is also increasing. When people who wear glasses eat, go from a cold place to a hot place, exhale too much hot air in rainy and snowy weather, or go out with masks, the water vapor in the air will condense into tiny water droplets and adhere to the lenses when it contacts the cold glass, PC or resin lenses, thus forming a layer of fog on the lenses. This phenomenon also exists on car windows, helmet covers, and lenses of various digital products. This phenomenon is detrimental to people's lives and even personal safety.
[0003] According to the patent with publication number CN 113774671 B, an anti-fog treatment agent, an anti-fog glasses cloth and a preparation method thereof are proposed. The anti-fog treatment agent is composed of the following raw materials: polyester fiber finishing agent, anti-fog microcapsules, emulsifier and penetrant; the core material of the anti-fog microcapsules is formed by stirring and dispersing titanium dioxide, acrylate monomers and turpentine, and the wall material is aminated sulfonated alkali lignin. The anti-fog treatment agent prepared in this application can form an anti-fog layer on the ultrafine fiber base cloth. When the anti-fog glasses cloth is rubbed against materials such as lenses, the anti-fog treatment agent on the anti-fog glasses cloth is partially transferred to the lenses. The outer wall material of the anti-fog microcapsules is decomposed under the action of light, and the loaded anti-fog oil in the internal core material can quickly solidify into a film under visible light, forming an anti-fog film on the surface of the lens, which plays an efficient and long-lasting anti-fog effect.
[0004] The conventional way to deal with this mirror fogging phenomenon is to wipe it with a paper towel or cloth. However, the traditional wiping cloth has a poor effect on fogging treatment and cannot be used for a long time. Often, fog will form again after wiping for a period of time. In addition, the anti-fog effect of the traditional wiping cloth may gradually weaken after repeated use.
[0005] Therefore, those skilled in the art have proposed an anti-fog cloth for lenses and a preparation method thereof to solve the problems raised by the background art.
[0006] The above information disclosed in this background technology is only used to increase the understanding of the background technology of the present invention and therefore, it may include information that does not constitute the prior art known to ordinary technicians in this field. Summary of the invention
[0007] The object of the present invention is to provide an anti-fog cloth for lenses and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A lens anti-fog cloth, comprising:
[0010] A cloth surface mechanism, the cloth surface mechanism comprising a cleaning cloth body, the cleaning cloth body comprising a sea-island fiber layer and a plurality of serrated protrusions arranged on the cleaning cloth body, and a surfactant is attached to the cleaning cloth body;
[0011] The processing mechanism includes an anti-fog layer and an antibacterial layer arranged on the cleaning cloth body.
[0012] Preferably, the size of the cleaning cloth body is 15 cm×15 cm.
[0013] Preferably, a nameplate hot stamping area is provided on one surface of the cleaning cloth body.
[0014] Preferably, a method for preparing an anti-fog cloth for lenses comprises the following steps:
[0015] S1 Fabric production: Collect raw materials and weave them into sea island silk fabric, and then pre-treat the finished fabric;
[0016] S2 Fabric cutting: Cut the pre-treated sea-island silk fabric according to the predetermined size, and cut the four sides of the fabric to form evenly distributed serrated protrusions;
[0017] S3 anti-fog treatment: prepare anti-fog agent and combine the prepared anti-fog agent with the sea island silk fabric surface by immersion method;
[0018] S4 antibacterial treatment: prepare antibacterial agent and use coating film forming method to form antibacterial coating on the surface of sea-island silk fabric;
[0019] S5 Service Life Test: Use the finished lens cleaning cloth as a test sample, wipe it on frosted glass and glass with bacteria, and judge whether the lens cleaning cloth can continue to be reused based on the degree of fog removal on the glass and the amount of residual bacteria.
[0020] Preferably, in step S1, during the production process of the fabric, the island silk fabric is made of a mixed weaving of silk and seaweed fiber in a ratio of 2:1, and sea clams, freshwater clams and abalone are used as raw materials. Through chemical and physical treatment, fibers are extracted and processed. Specifically, the processing steps include raw material processing, fiber extraction and weaving processing. The fiber density of the island silk is 0.05D.
[0021] Preferably, in step S1, during the fabric production process, before manufacturing the island silk, the fiber raw material is immersed in a chemical raw material, heated to 95 degrees Celsius, the hydrocarbons in the raw material are cracked to generate new fibers, and then processed through steam injection and chute drawing to produce the island silk.
[0022] Preferably, in step S1, during the fabric production process, pretreatment of the sea-island silk fabric includes washing, bleaching, drying, dyeing and printing.
[0023] Preferably, in step S3, in the anti-fog treatment operation, 10 parts of sodium dodecyl sulfate, 15 parts of sodium alkyl sulfosuccinate, 10 parts of propylene glycol, 20 parts of ethanol, 25 parts of glycerol, 30 parts of water and 15 parts of a binder are taken, and stirred at 80 degrees Celsius to prepare an anti-fog agent, wherein the binder is prepared by dissolving polyvinyl pyrrolidone and ethylene glycol in distilled water, stirring and dissolving, and precipitating. The sea island silk is immersed in the prepared anti-fog agent, the immersion temperature is 85 degrees Celsius, the immersion time is 50 minutes, and the number of immersions is 5 times.
[0024] Preferably, in step S4, in the antibacterial treatment operation, polyvinyl alcohol is used as the base film, and the magnetron sputtering process is used to uniformly adhere the metallic silver to the base film, and the adhesion thickness of the metallic silver on the base film is 1000nm. The base film with the attached silver film is immersed in deionized water to form a nanosilver film, wherein the immersion temperature is controlled at 95 degrees Celsius, and then the nanosilver film is dehydrated to obtain an antibacterial agent, and the nanosilver film is coated on the surface of the sea island silk, and immersed in an environment of 160 degrees Celsius for 5 minutes, and then the finished product is dehydrated and dried.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention provides a cleaning cloth body with a surfactant, and the cleaning cloth body has an anti-fog layer and an antibacterial layer. The cloth surface made of sea-island fibers is soft and will not scratch the lens, and has good anti-static properties and is not easy to generate static electricity, which brings convenience for daily use. At the same time, the sea-island fibers also have good durability and can maintain a long service life. Compared with traditional lens cloths, the present invention can provide more uses and save costs. The provision of the anti-fog layer and the antibacterial layer can provide the lens cloth with anti-fog and antibacterial functions, and can effectively remove fog and bacteria on the lens when wiping, and the duration is long, and there is no need to wipe repeatedly in a short period of time.
[0027] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present invention will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the three-dimensional structure of the present invention;
[0029] Figure 2 is a cross-sectional view of the cleaning cloth body of the present invention;
[0030] Figure 3 This is a schematic diagram of the explosion structure of the cleaning cloth body of the present invention;
[0031] Figure 4 It is a flow chart of the preparation method of the present invention.
[0032] In the figure: 1. Cleaning cloth body; 2. Serrated protrusions; 3. Nameplate hot stamping area; 4. Anti-fog layer; 5. Antibacterial layer; 6. Sea island fiber layer. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Embodiment 1:
[0035] See also Figure 1-Figure 3 As shown, a lens anti-fog cloth comprises:
[0036] The cloth surface mechanism comprises a cleaning cloth body 1, the cleaning cloth body 1 comprises a sea-island fiber layer 6 and a plurality of sawtooth protrusions 3 arranged on the cleaning cloth body 1, and a surfactant is attached to the cleaning cloth body 1;
[0037] The processing mechanism includes an anti-fog layer 4 and an antibacterial layer 5 arranged on the cleaning cloth body 1.
[0038] Specifically, the size of the cleaning cloth body 1 is 15 cm×15 cm.
[0039] Specifically, a nameplate hot stamping area 3 is provided on one surface of the cleaning cloth body 1 .
[0040] As can be seen from the above, the device is provided with a cleaning cloth main body 1 with a surfactant, and the cleaning cloth main body 1 has an anti-fog layer 4 and an antibacterial layer 5. The cloth surface made of sea island fibers is soft and will not scratch the lens, and has good anti-static properties and is not easy to generate static electricity, which brings convenience for daily use. At the same time, the sea island fibers also have good durability and can maintain a long service life. Compared with traditional lens cloths, the present invention can provide more times of use and save costs. The setting of the anti-fog layer 4 and the antibacterial layer 5 can provide the lens cloth with anti-fog and antibacterial functions, and can effectively remove fog and bacteria on the lens when wiping, and the duration is long, and there is no need to wipe repeatedly in a short time.
[0041] See also Figure 4 As shown, a method for preparing an anti-fog cloth for lenses comprises the following steps:
[0042] S1 Fabric production: Collect raw materials and weave them into sea island silk fabric, and then pre-treat the finished fabric;
[0043] S2 Fabric cutting: Cut the pre-treated sea-island silk fabric according to the predetermined size, and cut the four sides of the fabric to form evenly distributed serrated protrusions, which can fully clean the gaps in the frame of the lens;
[0044] S3 anti-fog treatment: prepare anti-fog agent and combine the prepared anti-fog agent with the sea island silk fabric surface by immersion method;
[0045] S4 antibacterial treatment: prepare antibacterial agent and use coating film forming method to form antibacterial coating on the surface of sea-island silk fabric;
[0046] S5 Service Life Test: Use the finished lens cleaning cloth as a test sample, wipe it on frosted glass and glass with bacteria respectively, and judge whether the lens cleaning cloth can continue to be reused based on the degree of fog removal on the glass and the amount of residual bacteria. The quality of the finished product can be guaranteed through repeated tests.
[0047] Specifically, in step S1, during the production process of the fabric, the sea island silk fabric is made of a mixed textile of silk and seaweed fiber in a ratio of 2:1, and sea clams, freshwater clams and abalone are used as raw materials. Through chemical and physical treatment, the fibers are extracted and processed. Specifically, the steps of raw material processing, fiber extraction and textile processing are required. The fiber density of the sea island silk is 0.05D.
[0048] Specifically, in step S1, during the fabric production process, before manufacturing the island-in-sea fibers, the fiber raw materials are immersed in chemical raw materials and heated to 95 degrees Celsius to crack the hydrocarbons in the raw materials to generate new fibers, which are then processed through steam injection and chute drawing to produce island-in-sea fibers.
[0049] Specifically, in step S1, during the fabric production process, the pretreatment of the sea-island silk fabric includes washing, bleaching, drying, dyeing and printing.
[0050] Specifically, in step S3, in the anti-fog treatment operation, 10 parts of sodium dodecyl sulfate, 15 parts of sodium alkyl sulfosuccinate, 10 parts of propylene glycol, 20 parts of ethanol, 25 parts of glycerol, 30 parts of water and 15 parts of a binder are taken, and stirred at 80 degrees Celsius to prepare an anti-fog agent, wherein the binder is obtained by dissolving polyvinyl pyrrolidone and ethylene glycol in distilled water, stirring and dissolving, and precipitating. The sea island silk is soaked in the prepared anti-fog agent, the soaking temperature is 85 degrees Celsius, the soaking time is 50 minutes, and the number of soaking times is 5 times. The good film-forming property of polyvinyl pyrrolidone is utilized, and it is easily soluble in water, insoluble in certain organic media, and the film is transparent, does not affect the original color, can improve the gloss and dispersibility of the pigment, and also has good adhesion. The raw materials of the anti-fog agent can be tightly bonded together, thereby improving the stability of the anti-fog agent, and can be loaded on the fiber fabric, so that when the lens encounters water vapor, it will not condense into small droplets, but will be completely spread out to form a transparent water film, thereby achieving an anti-fog effect.
[0051] Specifically, in step S4, in the antibacterial treatment operation, polyvinyl alcohol is used as the base film, and the magnetron sputtering process is used to uniformly adhere metallic silver to the base film, and the adhesion thickness of the metallic silver on the base film is 1000nm. The base film with the attached silver film is immersed in deionized water to form a nanosilver film, wherein the immersion temperature is controlled at 95 degrees Celsius, and then the nanosilver film is dehydrated to obtain an antibacterial agent, and the nanosilver film is coated on the surface of the sea island silk, and immersed in an environment of 160 degrees Celsius for 5 minutes, and then the finished product is dehydrated and dried.
[0052] As can be seen from the above, the present invention uses sea-island silk as the cloth material, and utilizes its good air permeability and moisture absorption to quickly wipe off water stains on the lens. The sea-island silk also has good anti-static properties and is not easy to generate static electricity. The good durability can keep the lens cloth for a long time, thereby improving the use experience. The anti-fog agent composed of a mixture of ethanol, glycerol and water can be loaded on the fiber fabric of the glasses cloth, so that the lens will not condense into small droplets when encountering water vapor, but will be completely spread out to form a transparent water film, thereby achieving an anti-fog effect. In addition, by setting a nano-silver film, it can penetrate the cell membrane of bacteria, so that the metal content in the bacterial cells surges, thereby causing metal poisoning. At the same time, silver ions can destroy the gene chain of bacterial genetic material so that it cannot continue to proliferate, and its proteins and lipids will also be damaged, thereby affecting the energy intake of bacteria, thereby achieving a good sterilization effect.
[0053] The standard parts used in the present invention can all be purchased from the market, and the special-shaped parts can be customized according to the description and the drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the prior art. The machinery, parts and equipment all adopt conventional models in the prior art, and the circuit connection adopts the conventional connection method in the prior art, which will not be described in detail here. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0054] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0055] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0056] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0057] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0058] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A lens anti-fog cloth, characterized in that: include: A cloth surface mechanism, the cloth surface mechanism comprising a cleaning cloth body (1), the cleaning cloth body (1) comprising a sea-island fiber layer (6) and a plurality of sawtooth protrusions (3) arranged on the cleaning cloth body (1), and a surfactant is attached to the cleaning cloth body (1); The processing mechanism comprises an anti-fog layer (4) and an antibacterial layer (5) arranged on a cleaning cloth body (1).
2. The anti-fog cloth for lenses according to claim 1, characterized in that: The size of the cleaning cloth body (1) is 15 cm×15 cm.
3. The anti-fog cloth for lenses according to claim 1, characterized in that: A nameplate hot stamping area (3) is provided on one surface of the cleaning cloth body (1).
4. The method for preparing an anti-fog cloth for lenses according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1 Fabric production: Collect raw materials and weave them into sea island silk fabric, and then pre-treat the finished fabric; S2 Fabric cutting: Cut the pre-treated sea-island silk fabric according to the predetermined size, and cut the four sides of the fabric to form evenly distributed serrated protrusions; S3 anti-fog treatment: prepare anti-fog agent and combine the prepared anti-fog agent with the sea island silk fabric surface by immersion method; S4 antibacterial treatment: prepare antibacterial agent and use coating film forming method to form antibacterial coating on the surface of sea-island silk fabric; S5 Service Life Test: Use the finished lens cleaning cloth as a test sample, wipe it on frosted glass and glass with bacteria, and judge whether the lens cleaning cloth can continue to be reused based on the degree of fog removal on the glass and the amount of residual bacteria.
5. The method for preparing an anti-fog cloth for lenses according to claim 4, characterized in that: In step S1, during the production process of the fabric, the sea island silk fabric is made of silk and seaweed fiber mixed in a ratio of 2:1, and sea clams, freshwater clams and abalone are used as raw materials. Through chemical and physical treatment, fibers are extracted and processed. Specifically, the steps of raw material processing, fiber extraction and textile processing are required. The fiber density of the sea island silk is 0.03-0.05D.
6. The method for preparing an anti-fog cloth for lenses according to claim 4, characterized in that: In step S1, during the fabric production process, before manufacturing the island-in-the-sea fibers, the fiber raw materials are immersed in chemical raw materials and heated to 80-95 degrees Celsius to crack the hydrocarbons in the raw materials to generate new fibers, which are then processed by steam injection and chute drawing to produce the island-in-the-sea fibers.
7. The method for preparing an anti-fog cloth for lenses according to claim 4, characterized in that: In step S1, during the fabric production process, the pretreatment of the sea-island silk fabric includes washing, bleaching, drying, dyeing and printing.
8. The method for preparing an anti-fog cloth for lenses according to claim 4, characterized in that: In step S3, in the anti-fog treatment operation, 8-10 parts of sodium dodecyl sulfate, 10-15 parts of sodium alkyl sulfosuccinate, 5-10 parts of propylene glycol, 15-20 parts of ethanol, 20-25 parts of glycerol, 27-30 parts of water and 10-15 parts of a binder are taken, and stirred at 80 degrees Celsius to prepare an anti-fog agent, wherein the binder is prepared by dissolving polyvinyl pyrrolidone and ethylene glycol in distilled water, stirring and dissolving, and precipitating. The sea island silk is soaked in the prepared anti-fog agent, the soaking temperature is 70-85 degrees Celsius, the soaking time is 30-50 minutes, and the number of soaking times is 3-5 times.
9. The method for preparing an anti-fog cloth for lenses according to claim 4, characterized in that: In step S4, in the antibacterial treatment operation, polyvinyl alcohol is used as the base film, and the magnetron sputtering process is used to uniformly adhere the metallic silver to the base film, and the adhesion thickness of the metallic silver on the base film is 20nm-2000nm. The base film with the attached silver film is immersed in deionized water to form a nanosilver film, wherein the immersion temperature is controlled at 70-95 degrees Celsius, and then the nanosilver film is dehydrated to obtain an antibacterial agent, and the nanosilver film is coated on the surface of the sea island silk, and immersed in an environment of 130-160 degrees Celsius for 3-5 minutes, and then the finished product is dehydrated and dried.
Citation Information
Patent Citations
Anti-fog agent, an anti-fog eyeglass cloth and its preparation method
CN113774671B