Asphalt mechanical property optimization method based on asphaltene content regulation and control
Through asphalt component extraction-remix technology and performance testing, the asphalt content is adjusted and the asphalt performance is optimized, the problem of the use of modifiers in the prior art is solved, and the performance improvement and cost reduction of asphalt materials are achieved.
Patent Information
- Application Number
- CN202410963782.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the optimization of asphalt performance by adding modifiers has problems such as overall unevenness, poor modification effect and increased cost, and it is difficult to effectively regulate the impact of asphaltene components on asphalt performance.
Through asphalt component extraction-relocation technology, the asphalt content is adjusted, and the high-temperature, medium-temperature and low-temperature performance of asphalt is tested using indicators such as rut factor, G-R parameters, creep stiffness modulus and creep rate, and the sensitive factor is calculated and the peak value is performed. Fit to determine the optimal asphaltene content to optimize the asphalt mechanical properties.
It has achieved the optimization of asphalt material performance by adjusting the asphalt content, avoiding the use of modifiers, reducing production costs, and avoiding the compatibility differences between modifiers and asphalt raw materials, providing a new theoretical basis and calculation method. .
Smart Images

Figure CN118913958A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road asphalt materials, and specifically discloses a method for optimizing asphalt mechanical properties based on asphaltene content regulation. Background Art
[0002] Asphalt is a widely used petroleum derivative product, mainly used in road construction, roof waterproofing, bridge paving and other engineering purposes. It is a complex mixture composed of a variety of organic molecules. According to their polarity, it can be divided into four components: saturated hydrocarbons, aromatic hydrocarbons, colloids and asphaltenes. Saturated hydrocarbons, aromatic hydrocarbons and colloids are classified as soft asphaltene. Asphaltene, as the most polar component, is the only component insoluble in n-heptane. Its content and characteristics have a decisive influence on the performance of asphalt. With the gradual increase in the performance requirements of asphalt in road engineering, in-depth research on the role of asphaltene in asphalt has become the key to optimizing asphalt materials and improving their performance.
[0003] Due to the complexity of the traditional asphalt component separation process, current research on asphaltene components only discusses the correlation between changes in asphaltene content and changes in asphalt performance under certain specific physicochemical conditions (such as aging or modification). Since the contents of the four components often change dynamically at the same time during the physicochemical process, the interaction between asphaltene and other components is also in a dynamic state. It is difficult to clarify the role of changes in asphaltene content in the change of asphalt performance in this process, resulting in the inability to quantitatively evaluate the impact of the content of a single asphaltene component on asphalt performance.
[0004] In addition, the current research on asphalt performance optimization methods is mostly focused on modifying asphalt by adding modifiers, but this method not only increases production costs, but also has potential compatibility issues. For example, the segregation or agglomeration of the modifier makes the modified asphalt uneven as a whole, resulting in poor modification effect of the modifier. Therefore, designing a method to optimize the mechanical properties of asphalt by controlling the asphalt component variables is of great significance for the use of road asphalt. Summary of the invention
[0005] In view of the prior art that optimizes asphalt performance by adding modifiers, there are still problems such as overall unevenness of modified asphalt, poor modification effect and increased cost. The present invention provides a method for optimizing asphalt mechanical properties based on regulating asphaltene content.
[0006] To achieve this object of the invention, the present invention provides the following technical solutions:
[0007] The first aspect of the present invention provides a method for optimizing the mechanical properties of asphalt based on asphaltene content regulation, comprising the following steps:
[0008] S1. extracting asphalt components and re-mixing to prepare re-mixed asphalt;
[0009] S2. Test the high-temperature, medium-temperature and low-temperature properties of the back-mixed asphalt. Use the rutting factor G* / sinδ to characterize the high-temperature anti-rutting ability of the back-mixed asphalt; use the GR parameter to characterize the medium-temperature fatigue performance of the back-mixed asphalt; use the creep stiffness modulus S and creep rate m to characterize the low-temperature crack resistance of the back-mixed asphalt;
[0010] S3. Calculate the sensitivity factor D of each indicator according to the formula A , where the formula is A n and A n~1 are the values of the performance index A of two adjacent back-mixed asphalts with higher asphaltene content and lower asphaltene content, respectively. A is the average value of the rutting factor G* / sinδ, the average value of the GR parameter, the average value of the creep stiffness modulus S or the creep rate m;
[0011] S4, through the sensitivity factor D A By peak fitting with the asphaltene content in the re-mixed asphalt, the most sensitive or least sensitive content of the high-temperature, medium-temperature and low-temperature performance of the re-mixed asphalt to the asphaltene content in the re-mixed asphalt can be obtained. According to the triangle circumcenter theorem and the average value method, the optimal asphaltene content in the re-mixed asphalt can be comprehensively determined according to the index requirements of high-temperature, medium-temperature or low-temperature performance.
[0012] Compared with the prior art, the present invention first obtains the re-matched asphalt through the asphalt component extraction-re-matching technology. The re-matched asphalt is obtained by changing the asphalt content on the basis of determining the soft asphalt, and the variable is only the asphalt content, which is convenient for determining the influence of the asphalt content on the comprehensive mechanical properties of asphalt. The present invention also determines the high-temperature, medium-temperature and low-temperature properties of the re-matched asphalt through dynamic shear rheology tests, and characterizes the high-temperature anti-rutting ability of the re-matched asphalt with the rutting factor, the medium-temperature fatigue performance of the re-matched asphalt with the GR parameter, and the low-temperature anti-cracking performance of the re-matched asphalt with the creep stiffness modulus and creep rate; these three parameters can be used as performance test indicators to fully characterize the mechanical properties of the re-matched asphalt obtained by the present invention at different temperatures under the condition of only changing the asphalt content. Then, the present invention substitutes the relevant data of high temperature, medium temperature and low temperature obtained from the experiment into the formula of asphaltene content sensitivity factor to calculate the most sensitive or least sensitive content of the returned asphalt at different asphaltene contents to the asphalt content at high temperature, medium temperature and low temperature, thereby determining the sensitivity of asphalt to asphalt content under different performance requirements of high temperature, medium temperature or low temperature, and finally determines the asphalt content with the best comprehensive performance of asphalt through peak fitting.
[0013] The present invention can obtain asphalt materials with the best comprehensive performance only by adjusting the asphaltene content, without adding any modifiers, greatly reducing the cost of improving the performance of asphalt materials, and avoiding the problems of poor compatibility between modifiers and asphalt raw materials and uneven modification. The technical solution of the present invention effectively solves the problem of adding modifiers to optimize asphalt performance in the prior art, but still has the problems of overall uneven modified asphalt, poor modification effect and increased cost, and provides a new theoretical basis and calculation method for the selection and optimization of asphalt materials.
[0014] Preferably, the specific preparation method of the re-mixed asphalt comprises the following steps:
[0015] Step a, mixing asphalt and alkyl solvent evenly, stirring for 22h to 26h under vacuum conditions to obtain an asphalt mixture;
[0016] Step b, filtering the asphalt mixture and vacuum drying to obtain asphaltene and soft asphaltene;
[0017] Step c, dissolving asphaltene with different contents in organic solvents to obtain a series of asphaltene solutions; adding soft asphaltene to the series of asphaltene solutions, mixing them evenly, and drying them to obtain the mixed asphalt.
[0018] Further preferably, in step a, the alkyl solvent is n-heptane.
[0019] Further preferably, in step a, the mass ratio of the asphalt to the alkyl solvent is 1:28 to 1.5:45.
[0020] Further preferably, in step a, the rotation speed of the low-speed stirring is 180 r / min to 220 r / min.
[0021] Further preferably, in step b, the pore size of the filter for vacuum filtration is 0.15 μm to 0.25 μm.
[0022] Further preferably, in step b, the vacuum drying temperature is 130° C. to 140° C., the vacuum drying pressure is -180 Pa to -130 Pa, and the vacuum drying time is 22 h to 26 h.
[0023] Further preferably, in step c, the organic solvent is trichloroethylene.
[0024] Further preferably, in step c, the mass ratio of the asphaltene to the organic solvent is 1:135-1.1:150.
[0025] Further preferably, in step c, the drying temperature is 130° C. to 140° C., the drying pressure is -230 Pa to -130 Pa, and the vacuum drying time is 22 h to 26 h.
[0026] Preferably, in S2, the calculation formula of the GR parameter is: Where G* is the complex shear modulus; δ is the phase angle; G* and δ are the values corresponding to an angular frequency of 0.005 rad / s.
[0027] In summary, the present invention firstly obtains the re-matched asphalt through the asphalt component extraction-re-matching technology, and then determines the high temperature, medium temperature and low temperature performance of the re-matched asphalt through dynamic shear rheology test, and then substitutes the test data into the sensitive factor formula to calculate the most sensitive / least sensitive content under different asphalt contents, and determines the asphaltene content with the best comprehensive performance of asphalt through peak fitting. The technical solution provided by the present invention can obtain the asphalt material with the best comprehensive performance only by adjusting the asphaltene content, without adding any modifier, which effectively solves the purpose of optimizing the asphalt performance by adding modifiers in the prior art, but there are still problems such as overall unevenness of modified asphalt, poor modification effect and increased cost, which provides a new theoretical basis and calculation method for the selection and optimization of asphalt materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The pictures of asphaltene and asphaltene are shown in Figure 1. Figure 1 (a) Black asphaltene particles; Figure 1 (b) is yellow-brown soft asphalt;
[0029] Figure 2 is the asphaltene content and sensitivity factor D 车辙因子 and D G-R The peak fitting diagram of
[0030] Figure 3 It is the fitting curve diagram of asphaltene content, rutting factor, GR parameter, creep stiffness modulus S and creep rate m. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment provides a method for optimizing the mechanical properties of asphalt based on asphaltene content regulation, which specifically includes the following contents:
[0034] S1. Select 70# matrix asphalt, take 0.4g of asphalt sample with a scraper and put it into a vacuum-dedicated reaction bottle, and put a magnetic rotor in it. Use a measuring cylinder to measure 25mL of n-heptane, pour it into a 100mL reaction bottle, cover the reaction bottle cap, extract the air in the reaction bottle, and form a vacuum in the bottle; place the reaction bottle on a magnetic stirrer, set the stirring speed to 200r / min, stir for 2h, and put the stirred mixed solution into a syringe connected to a membrane filter at one end, the pore size of the filter membrane is 0.22μm, and connect the other end of the membrane filter to a vacuum filtration device, and vacuum filter the mixed solution. The soft asphaltene dissolved in the n-heptane solvent will penetrate through the filter membrane into the glass tube below, and the insoluble asphaltene will be retained above the filter membrane; after the filtration is completed, remove the filter membrane, place it in a glass desiccator and let it stand for 24h to complete the drying of the asphaltene, then open the filter membrane, take out the dried asphaltene on the filter paper and recycle it;
[0035] S2. Place the filtered soft asphaltene solution in a vacuum drying oven, evacuate the drying oven to a vacuum pressure of -150Pa, set the drying temperature to 105°C, dry for 24 hours, complete the drying of the soft asphaltene, and pour the dried soft asphaltene into a beaker container for recovery. Repeat the above recovery method several times until 5g of asphaltene and 30g of soft asphaltene are recovered.
[0036] S3. Weigh 0.2 g of asphaltene and put it into a vacuum reaction bottle, and then put a magnetic rotor in it, add 20 mL of trichloroethylene, cover the bottle cap, place the reaction bottle on a magnetic stirrer, set the speed to 200 r / min, stir for 1 hour, so that the asphaltene is fully dissolved, and an asphaltene-trichloroethylene solution is obtained; after the stirring is completed, 4.8 g of soft asphaltene and 30 mL of trichloroethylene are added to the asphaltene-trichloroethylene solution, the speed is set to 200 r / min, and stirred for 1 hour to dissolve the soft asphaltene, and the asphaltene and the soft asphaltene are mixed at the same time; the mixed solution is placed in a vacuum drying oven, the drying oven is evacuated to a vacuum pressure of -180 Pa, the drying temperature is set to 105°C, and it is dried for 24 hours, and the trichloroethylene solvent is evaporated to dryness, and the preparation of the re-matched asphalt with an asphaltene content of 4% is completed.
[0037] S4. According to the above process, 0.4g, 0.6g, 0.8g and 1g of asphaltene are weighed respectively, and 4.6g, 4.4g, 4.2g and 4g of soft asphaltene are weighed correspondingly to complete the preparation of re-mixed asphalt with asphaltene content of 8%, 12%, 16% and 20%.
[0038] Test method:
[0039] A dynamic shear rheometer was used to test the high-temperature performance of the re-mixed asphalt samples. A 25mm metal parallel plate fixture was selected, and the distance between the two metal plates was set to 1mm. The re-mixed asphalt samples were subjected to frequency scanning tests at temperatures of 35°C, 45°C and 55°C. The strain was 1%, and the angular frequency was 10rad / s. The corresponding complex shear modulus G* and phase angle δ were used to calculate the rutting factor of the sample, and the average rutting factor of the re-mixed asphalt at three temperatures was further calculated.
[0040] The medium-temperature performance of the re-mixed asphalt sample was tested using a dynamic shear rheometer. An 8mm metal parallel plate fixture was selected, and the distance between the two metal plates was set to 2mm. The re-mixed asphalt sample was subjected to a frequency sweep test at 5°C, 15°C, and 25°C, with a strain of 1%. The master curve was constructed, and the complex shear modulus and phase angle corresponding to the angular frequency of 0.005rad / s at 15°C were obtained by interpolation, and the GR parameters were calculated. The GR parameters can be calculated using the following formula:
[0041]
[0042] Where G* is the complex shear modulus; δ is the phase angle; G* and δ are the values corresponding to an angular frequency of 0.005 rad / s.
[0043] A dynamic shear rheometer was used to test the low-temperature performance of the re-mixed asphalt samples. A 4mm metal parallel plate fixture was selected and the distance between the two metal plates was set to 2mm. Frequency scanning tests were carried out on the re-mixed asphalt samples at -6℃, -12℃ and -18℃ with a strain of 0.1%. The average values of the creep stiffness modulus S and creep rate m of the re-mixed asphalt at three temperatures were calculated.
[0044] For a total of 5 asphalt samples with asphaltene content of 4%, 8%, 12%, 16% and 20%, the average values of rutting factor at 35°C, 45°C and 55°C, GR parameter, creep stiffness modulus S and creep rate m at -6°C, -12°C and -18°C were respectively selected and substituted into the sensitivity factor formula to calculate the sensitivity of different properties of the asphaltene content. The peak values of sensitivity and asphaltene content were fitted to solve the most sensitive / least sensitive points of different properties to asphaltene content, and the asphaltene content that makes the asphaltene content optimal was determined based on the average value method. The results are shown in Table 1 and Figure 2 shown.
[0045] Then, the relationship between asphaltene content and high temperature, medium temperature and low temperature performance indicators is established, and the relationship expression between asphaltene content and different performance indicators is constructed by regression fitting method, and the optimal asphaltene content obtained is substituted into each relationship expression, where the asphaltene content-rutting factor relationship is y=877x 1.45; The asphaltene content-GR parameter relationship is y = 0.31 + 0.011e (x-0.014) / 0.019 ; The asphaltene content-creep stiffness modulus relationship is y = 32.93e (x / 0.08)-6.87 The asphaltene content-creep rate relationship is y=-2.69x+0.75. According to the relationship expression, it is verified that the performance indicators of the re-mixed asphalt corresponding to the optimal asphaltene content obtained by solving the solution meet the use requirements. The results are as follows Figure 3 shown.
[0046] Table 1 Calculation results of sensitivity of different performance indicators to asphaltene content
[0047] project 4% Asphaltene 8% Asphaltene 12% Asphaltene 16% Asphaltene 20% Asphaltene <![CDATA[D 车辙因子 ]]> 1.80 2.17 0.76 0.48 0.41 <![CDATA[D G-R ]]> 2.88 2.42 4.69 5.69 6.97 <![CDATA[D S ]]> 0.79 0.67 0.71 0.71 0.59 <![CDATA[D m ]]> -0.23 -0.15 -0.19 -0.18 -0.19
[0048] It can be seen from Table 1 that the sensitivity of the average rutting factor and GR parameter of the re-mixed asphalt to the asphaltene content has an obvious turning point range, while the creep stiffness modulus S and creep rate m have a small fluctuation in sensitivity to the asphaltene content and there is no obvious turning point range.
[0049] Based on the data in Table 1, the present invention has a significant effect on the D 车辙因子 and D G-R Peak fitting was performed and the fitting results are shown in Figure 2 Based on the fitting results, it can be calculated that the asphaltene content corresponding to the point where the asphalt high temperature performance is most sensitive to the asphaltene content is 6.18%, and the asphaltene content corresponding to the point where the asphalt fatigue performance is least sensitive to the asphaltene content is 6.26%. The two are very close, so the middle value of 6.22% is taken as the optimal asphaltene content.
[0050] In order to verify that when the asphaltene content is 6.22%, the various properties of the re-mixed asphalt meet the use requirements, the asphaltene content of 6.22% is substituted into the fitting curve of various properties of asphalt and asphaltene content, as shown in Figure 3 As shown. It can be obtained that the average value of G* / sinδ is 15.63kPa, the GR parameter is 0.45kPa, the average value of creep stiffness modulus S is 64.78MPa, and the average value of creep rate m is 0.58. It can be seen that when the asphaltene content is 6.22%, the high temperature, fatigue and low temperature properties of the asphalt are all good. Therefore, it can be considered that for a given 70# asphalt, when the asphaltene content: soft asphaltene content is 6.22%: 93.78%, the comprehensive performance of the back-matched asphalt is optimal.
[0051] Example 2
[0052] This embodiment provides a method for optimizing the mechanical properties of asphalt based on asphaltene content regulation, which specifically includes the following contents:
[0053] Select 90# matrix asphalt, take 0.4g asphalt sample with a scraper and put it into a vacuum special reaction bottle, and put a magnetic rotor, measure 20mL of n-heptane solvent with a measuring cylinder, pour it into the reaction bottle, cover the reaction bottle cap, extract the air in the reaction bottle, and form a vacuum in the bottle. Place the reaction bottle on a magnetic stirrer, set the stirring speed to 200r / min, stir for 24h, load the stirred mixed solution into a syringe connected to a membrane filter at one end, the pore size of the membrane is 0.22μm, connect the other end of the membrane filter to a vacuum filtration device, and vacuum filter the mixed solution. The soft asphaltene dissolved in the n-heptane solvent will penetrate the filter membrane into the glass tube below, and the insoluble asphaltene will be retained above the filter membrane. After the filtration is completed, the filter membrane is removed and placed in a glass dryer for 24h to complete the drying of the asphaltene. After that, the filter membrane is opened, the dried asphaltene on the filter paper is taken out and recovered. The filtered soft asphaltene solution was placed in a vacuum drying oven, the drying oven was evacuated, the temperature was set to 105°C, and the asphaltene was dried for 24 hours to complete the drying of the soft asphaltene. The dried soft asphaltene was poured into a beaker container for recovery. The above recovery method was repeated several times until 5g of asphaltene and 30g of soft asphaltene were recovered.
[0054] Weigh 0.25g of asphaltene into a vacuum reaction bottle, put it into a magnetic rotor, add 20mL of trichloroethylene solvent, cover the bottle cap, place the reaction bottle on a magnetic stirrer, set the speed to 200r / min, stir for 1h, and fully dissolve the asphaltene. After stirring, add 4.75g of soft asphaltene and 30mL of trichloroethylene solvent to the asphaltene-trichloroethylene solution, set the speed to 200r / min, stir for 1h, dissolve the soft asphaltene, and mix the asphaltene and soft asphaltene at the same time. Place the mixed solution in a vacuum drying oven, evacuate the drying oven, set the drying temperature to 105℃, leave it for 24h, evaporate the trichloroethylene solvent, and complete the preparation of the back-mixed asphalt with an asphaltene content of 5%. According to the above process, 0.5g, 0.75g, 1g, and 1.25g of asphaltene were weighed respectively, and 4.5g, 4.25g, 4g, and 3.75g of soft asphaltene were weighed correspondingly to complete the preparation of re-mixed asphalt with asphaltene content of 10%, 15%, 20%, and 25%.
[0055] The test method is consistent with that in Example 1 and will not be described again here.
[0056] Example 3
[0057] This embodiment provides a method for optimizing the mechanical properties of asphalt based on asphaltene content regulation, which specifically includes the following contents:
[0058] Select 70# matrix asphalt from different oil sources, take 0.4g of asphalt sample with a scraper and put it into a vacuum special reaction bottle, and put a magnetic rotor in it. Use a measuring cylinder to measure 23mL of n-heptane solvent, pour it into the reaction bottle, cover the reaction bottle cap, extract the air in the reaction bottle, and form a vacuum in the bottle. Place the reaction bottle on a magnetic stirrer, set the stirring speed to 200r / min, stir for 24h, and load the stirred mixed solution into a syringe connected to a membrane filter at one end. The pore size of the membrane is 0.22μm. Connect the other end of the membrane filter to a vacuum filtration device, and vacuum filter the mixed solution. The soft asphaltene dissolved in the n-heptane solvent will penetrate the filter membrane into the glass tube below, and the insoluble asphaltene will be retained above the filter membrane. After the filtration is completed, the filter membrane is removed and placed in a glass dryer for 24h to complete the drying of the asphaltene. After that, the filter membrane is opened, and the dried asphaltene on the filter paper is taken out and recovered. The filtered soft asphaltene solution was placed in a vacuum drying oven, the drying oven was evacuated, the temperature was set to 105°C, and the asphaltene was dried for 24 hours to complete the drying of the soft asphaltene. The dried soft asphaltene was poured into a beaker container for recovery. The above recovery method was repeated several times until 5g of asphaltene and 30g of soft asphaltene were recovered.
[0059] Weigh 0.3g of asphaltene into a vacuum reaction bottle, put it into a magnetic rotor, add 20mL of trichloroethylene solvent, cover the bottle cap, place the reaction bottle on a magnetic stirrer, set the speed to 200r / min, stir for 1h, and fully dissolve the asphaltene. After stirring, add 4.7g of soft asphaltene and 30mL of trichloroethylene solvent to the asphaltene-trichloroethylene solution, set the speed to 200r / min, stir for 1h, dissolve the soft asphaltene, and mix the asphaltene and soft asphaltene. Place the mixed solution in a vacuum drying oven, evacuate the drying oven, set the drying temperature to 105℃, dry for 24h, evaporate the trichloroethylene solvent, and complete the preparation of the back-matched asphalt with an asphaltene content of 5%. According to the above process, 0.6g, 0.9g, 1.2g, and 1.5g of asphaltene were weighed respectively, and 4.4g, 4.1g, 3.8g, and 3.5g of soft asphaltene were weighed correspondingly to complete the preparation of re-mixed asphalt with asphaltene content of 12%, 18%, 24%, and 30%.
[0060] The test method is consistent with that in Example 1 and will not be described again here.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for optimizing the mechanical properties of asphalt based on the regulation of asphaltene content. Features: The steps include: S1. extracting asphalt components and re-mixing to prepare re-mixed asphalt; S2. Test the high-temperature, medium-temperature and low-temperature properties of the back-mixed asphalt. Use the rutting factor G* / sinδ to characterize the high-temperature anti-rutting ability of the back-mixed asphalt; use the GR parameter to characterize the medium-temperature fatigue performance of the back-mixed asphalt; use the creep stiffness modulus S and creep rate m to characterize the low-temperature crack resistance of the back-mixed asphalt; S3. Calculate the sensitivity factor D of each indicator according to the formula A , where the formula is A n and A n~1 are the values of the performance index A of two adjacent back-mixed asphalts with higher asphaltene content and lower asphaltene content, respectively. A is the average value of the rutting factor G* / sinδ, the average value of the GR parameter, the average value of the creep stiffness modulus S or the creep rate m; S4, through the sensitivity factor D A By peak fitting with the asphaltene content in the re-mixed asphalt, the most sensitive or least sensitive content of the high-temperature, medium-temperature and low-temperature performance of the re-mixed asphalt to the asphaltene content in the re-mixed asphalt can be obtained. According to the triangle circumcenter theorem and the average value method, the optimal asphaltene content in the re-mixed asphalt can be comprehensively determined according to the index requirements of high-temperature, medium-temperature or low-temperature performance.
2. The method for optimizing asphalt mechanical properties based on asphaltene content control according to claim 1, Features: The specific preparation method of the re-mixed asphalt comprises the following steps: Step a, mixing asphalt and alkyl solvent evenly, stirring for 22h to 26h under vacuum conditions to obtain an asphalt mixture; Step b, filtering the asphalt mixture and vacuum drying to obtain asphaltene and soft asphaltene; Step c, dissolving asphaltene with different contents in organic solvents to obtain a series of asphaltene solutions; adding soft asphaltene to the series of asphaltene solutions, mixing them evenly, and drying them to obtain the mixed asphalt.
3. The method for optimizing asphalt mechanical properties based on asphaltene content control according to claim 2, Features: In step a, the alkyl solvent is n-heptane; and / or In step a, the mass ratio of the asphalt to the alkyl solvent is 1:28 to 1.5:45; and / or In step a, the stirring speed is 180 r / min to 220 r / min.
4. The method for optimizing asphalt mechanical properties based on asphaltene content control as claimed in claim 2, Features: In step b, the pore size of the vacuum filtration filter is 0.15 μm to 0.25 μm; and / or In step b, the vacuum drying temperature is 130° C. to 140° C., the vacuum drying pressure is -180 Pa to -130 Pa, and the vacuum drying time is 22 h to 26 h.
5. The method for optimizing asphalt mechanical properties based on asphaltene content control according to claim 2, Features: In step c, the organic solvent is trichloroethylene; and / or In step c, the mass ratio of the asphaltene to the organic solvent is 1:135-1.1:150; and / or In step c, the drying temperature is 130° C. to 140° C., the drying pressure is -230 Pa to -130 Pa, and the vacuum drying time is 22 h to 26 h.
6. The method for optimizing asphalt mechanical properties based on asphaltene content control according to claim 1, Features: In S2, the calculation formula of the GR parameter is: Where G* is the complex shear modulus; δ is the phase angle; G* and δ are the values corresponding to an angular frequency of 0.005 rad / s.
Citation Information
Cited By
Method for controlling mechanical property of asphalt in situ
CN120160872A