Preparation method and application of all-solid-state Ag / AgCl electrode
The all-solid-state Ag/AgCl electrode prepared by rapid sintering with a Joule heating device and graphene modification solves the problem of insufficient electrochemical performance in marine exploration, achieves electrode stability and reduces electrochemical noise, and is suitable for the field of marine exploration.
Patent Information
- Application Number
- CN202411165901.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
AI Technical Summary
The graphene-modified Ag/AgCl electrodes prepared by existing technologies have insufficient electrochemical performance in marine exploration, making it difficult to meet the needs of rapid deployment and real-time detection. Furthermore, conventional electrodes exhibit significant stability and electrochemical noise in deep-sea environments.
A Joule heating device was used for rapid sintering, combined with graphene modification, to prepare an all-solid-state Ag/AgCl electrode. Through steps such as light-shielded grinding, ball milling, pressing and drying, the temperature and time were controlled to increase the specific surface area and porosity and reduce electrochemical noise.
The prepared all-solid-state Ag/AgCl electrode has a small range, low electrochemical noise, and good stability, making it suitable for marine exploration. It also shortens the production time and is suitable for large-scale production.
Smart Images

Figure CN118914628A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemical electrode material preparation, and specifically relates to a preparation method and application of an all-solid-state Ag / AgCl electrode. Background Art
[0002] At present, ocean electric field detection is widely used in the fields of marine resource exploration and underwater weapon detection. The detection of ocean electric field mainly obtains signals by detecting the potential difference between electrodes. The deep sea environment requires that the electrodes should not only have low extremes and electrochemical noise, but also be able to work stably for a long time and avoid maintenance as much as possible. Conventional electrodes are difficult to cope with such a complex environment in the ocean, so it is urgent to develop and design an ocean detection electrode that meets the conditions.
[0003] The all-solid-state Ag / AgCl electrode prepared by tableting performs well among all electrodes. As an ideal non-polarizable electrode, the all-solid-state metal / parely soluble salt structure not only ensures the stability of the electrode structure, but also enables the reaction on the electrode to quickly reach equilibrium. Prior art (Study on the surface properties of graphene-modified Ag / AgCl electrodes_Li Hongxia) adds a certain amount of graphene to Ag and Ag Cl powders, and prepares graphene-modified Ag / AgCl electrodes by sintering. Electrochemical performance tests and electrode surface scanning electron microscopy tests are performed respectively. The fractal dimensional characteristics after adding different amounts of graphene are studied by fractal dimensional analysis of microstructure photos; Figure 3 It can be seen that the extreme stability time of 0%, 1%, and 3% graphene electrode samples is 24h, 5h, and 1h, respectively, and the extreme values are 0.3mV, 0.23mV, and 0.07mV, respectively. However, the demand for rapid deployment and real-time detection in ocean exploration places extremely high demands on the electrochemical performance of electrodes, so the electrochemical performance of electrodes prepared by existing technologies still has a lot of room for improvement. Summary of the invention
[0004] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing an all-solid-state Ag / AgCl electrode. The method uses a Joule heating device for rapid sintering, improves the firing process, shortens the firing time, saves energy, and precisely controls the temperature to achieve uniform heating.
[0005] Another object of the present invention is to provide an all-solid-state Ag / AgCl electrode provided by the above method. The electrode has certain pores, which increases the specific surface area of the electrode and has excellent electrochemical properties such as good stability, small range, and small electrochemical noise.
[0006] Another object of the present invention is to provide applications of the above-mentioned all-solid-state Ag / AgCl electrode.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for preparing an all-solid-state Ag / AgCl electrode comprises the following steps:
[0009] (1) Grind silver chloride into a fine powder in a dark environment;
[0010] (2) mixing silver chloride powder and ultrafine silver powder, adding graphene thereto, and then ball milling the mixed powder;
[0011] (3) After ball milling, the mixture is filtered out and dried;
[0012] (4) In a dark environment, take the dried powder, sieve it, pour it into a tableting mold, and perform preliminary pressing into shape;
[0013] (5) Compressing the preliminarily compressed sample more tightly by a tablet press;
[0014] (6) placing the sample in a Joule heating device for rapid sintering;
[0015] (7) After the fired electrode is polished, a wire is connected to the outside, and after packaging, it is placed in an acid solution for activation to obtain a graphene-doped all-solid-state Ag / AgCl electrode.
[0016] Furthermore, in step (1), the agglomerated silver chloride is ground into fine powder, the grinding time is 0.2-0.4h, and the whole process is performed in a dark environment.
[0017] Furthermore, in step (2), the molar ratio of the silver chloride powder to the ultrafine silver powder is 1:1, and graphene is added thereto to obtain a mixed powder with a graphene mass percentage of 3-5%; the mixed powder is placed in a ball mill, and anhydrous ethanol and agate beads of the same mass as the mixed powder are added; finally, the ball mill is placed in a planetary ball mill to ball mill the mixture, the ball milling speed is 300-500 r / min, and the ball milling time is 4-6 hours.
[0018] Furthermore, the drying temperature in step (3) is 50-80° C., and the drying time is 8 hours.
[0019] Furthermore, in step (4), the amount of powder filled in each tableting step is 0.25-0.35 g.
[0020] Furthermore, in step (5), the tablet press applies a pressure of 200-230 MPa to the powder, and the pressure holding time is 10-15 min.
[0021] Furthermore, in step (6), the Joule heating device is set at a temperature of 350-450° C., and the sintering time is 15-25 s.
[0022] Further preferably, the Joule heating device in step (6) is set at a temperature of 400° C. and a sintering time of 15 s.
[0023] Furthermore, the acid solution in step (7) is dilute hydrochloric acid with a concentration of 0.01 mol / L.
[0024] The all-solid-state Ag / AgCl electrode prepared by the above method has good stability, with a range as low as 0.052mV and electrochemical noise reduced to 3.15nV, and can be used in the field of ocean exploration.
[0025] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0026] 1. The method of the present invention increases the specific surface area and porosity of the electrode, reduces electrochemical noise and shortens the range stabilization time. The prepared electrode is suitable for the environment of weak electrical signals in the deep sea.
[0027] 2. The method of the present invention greatly reduces the time of firing electrodes, which is conducive to improving production efficiency. At the same time, the fast firing technology can accurately control the temperature and heat evenly. The prepared electrodes have small differences and good consistency, which is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the internal structure of the Joule heating device in the first embodiment of the present invention, wherein: 1. wire; 2. copper electrode; 3. graphite gasket; 4. sample; 5. quartz tube.
[0029] Figure 2 This is a schematic diagram of the internal structure of the Joule heating device in the second embodiment of the present invention, wherein: 1. wire; 2. copper electrode; 3. graphite felt; 4. sample.
[0030] Figure 3 It is a comparison chart of sintering time, porosity and specific surface area of electrodes prepared in Example 2 and Example 3. The rapid sintering in the figure represents Example 2, and the ordinary sintering represents Example 3.
[0031] Figure 4 3 is a comparison diagram of the range and electrochemical noise of the electrodes prepared in Example 2 and Example 3. The rapid sintering in the figure represents Example 2, and the ordinary sintering represents Example 3. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. The raw materials involved in the present invention can be purchased directly from the market. For process parameters not particularly noted, conventional techniques can be used.
[0033] Embodiment 1
[0034] This embodiment provides a method for rapidly preparing an all-solid-state Ag / AgCl electrode, and the specific steps are as follows:
[0035] 1) In a dark environment, grind the agglomerated silver chloride into a fine powder in an agate mortar for 0.2 h.
[0036] 2) Mix silver chloride powder and ultrafine silver powder in a molar ratio of 1:1, add a certain amount of graphene thereto, and obtain a mixed powder with a graphene mass percentage of 3%. Then put the mixed powder into a ball mill, add anhydrous ethanol and agate beads of the same mass as the mixed powder. Finally, put the ball mill into a planetary ball mill to ball mill the mixture at a speed of 300r / min for 6h.
[0037] 3) After the ball milling is completed, the mixture in the ball mill is sieved and placed in an oven for drying at 50°C for 8 hours.
[0038] 4) In a light-proof environment, take 0.25-0.35 g of the dried powder and pour it into a tableting mold for preliminary pressing.
[0039] 5) The preliminarily pressed sample is compressed more tightly by a tablet press, which applies a pressure of 200 MPa to the powder and maintains the pressure for 15 min.
[0040] 6) Place the sample into the Figure 1 The structure was rapidly sintered in a Joule heating device at a temperature of 400°C for 15 seconds.
[0041] 7) After the fired electrode is polished, a wire is connected to the outside, and after packaging, it is placed in a 0.01 mol / L dilute hydrochloric acid solution for activation to obtain a fully solid-state Ag / AgCl electrode.
[0042] Refer to the attached Figure 1 The Joule heating device used in the embodiment of the present invention includes a wire 1, a copper electrode 2, a graphite gasket 3, a sample 4, and a quartz tube 5. The wire 1 is connected to the copper electrode 2; the graphite gasket 3 is connected to the copper electrode 2; the sample 4 is sandwiched between two graphite gaskets 3; and the quartz tube 5 fixes the copper electrode 2, the graphite gasket 3, and the sample 4 together.
[0043] Embodiment 2
[0044] This embodiment provides a method for rapidly preparing an all-solid-state Ag / AgCl electrode, and the specific steps are as follows:
[0045] 1) In a dark environment, grind the agglomerated silver chloride into a fine powder in an agate mortar for 0.2 h.
[0046] 2) Mix silver chloride powder and ultrafine silver powder in a molar ratio of 1:1, add a certain amount of graphene thereto, and obtain a mixed powder with a graphene mass percentage of 3%. Then put the mixed powder into a ball mill, add anhydrous ethanol and agate beads of the same mass as the mixed powder. Finally, put the ball mill into a planetary ball mill to ball mill the mixture at a speed of 500r / min for 4h.
[0047] 3) After the ball milling is completed, the mixture in the ball mill is sieved and placed in an oven for drying at 60°C for 6 hours.
[0048] 4) In a light-proof environment, take 0.25-0.35 g of the dried powder and pour it into a tableting mold for preliminary pressing.
[0049] 5) The preliminarily pressed sample is compressed more tightly by a tablet press, which applies a pressure of 200 MPa to the powder and maintains the pressure for 15 min.
[0050] 6) Place the sample into the Figure 2 The structure was rapidly sintered in a Joule heating device at a temperature of 400°C for 15 seconds.
[0051] 7) After the fired electrode is polished, a wire is connected to the outside, and after packaging, it is placed in a 0.01 mol / L dilute hydrochloric acid solution for activation to obtain a fully solid-state Ag / AgCl electrode.
[0052] Refer to the attached Figure 2 The Joule heating device used in the embodiment of the present invention includes a wire 1, a copper electrode 2, a graphite felt 3, and a sample 4. The wire 1 is connected to the copper electrode 2; the sample 4 is sandwiched between two graphite felts 3; and the two graphite felts 3 are fixed by two copper electrodes 2.
[0053] Embodiment 3
[0054] This embodiment provides a conventional method for preparing a graphene-doped Ag / AgCl electrode. Except for the sintering process, the other processes are the same as those in the second embodiment. The specific steps are as follows:
[0055] 1) In a dark environment, grind the agglomerated silver chloride into a fine powder in an agate mortar for 0.2 h.
[0056] 2) Mix silver chloride powder and ultrafine silver powder in a molar ratio of 1:1, add a certain amount of graphene thereto, and obtain a mixed powder with a graphene mass percentage of 3%. Then put the mixed powder into a ball mill, add anhydrous ethanol and agate beads of the same mass as the mixed powder. Finally, put the ball mill into a planetary ball mill to ball mill the mixture at a speed of 500r / min for 4h.
[0057] 3) After the ball milling is completed, the mixture in the ball mill is sieved and placed in an oven for drying at 60°C for 6 hours.
[0058] 4) In a light-proof environment, take 0.25-0.35 g of the dried powder and pour it into a tableting mold for preliminary pressing.
[0059] 5) The preliminarily pressed sample is compressed more tightly by a tablet press, which applies a pressure of 200 MPa to the powder and maintains the pressure for 15 min.
[0060] 6) Place the sample in a muffle furnace, set the heating rate to 5°C / min, heat to 400°C and maintain the temperature for a period of time. The total heating time is 1.5 hours.
[0061] 7) After the fired electrode is polished, a wire is connected to the outside, and after packaging, it is placed in a 0.01 mol / L dilute hydrochloric acid solution for activation to obtain a fully solid-state Ag / AgCl electrode.
[0062] Experimental example:
[0063] 1. The electrode prepared by rapid sintering and the electrode prepared by ordinary sintering in Example 2 are immersed in a 3% mass concentration NaCl solution, and the deionized water is allowed to fully penetrate the pores inside the electrode by the immersion medium method. The mass of the electrode weighed in the air before immersion is m1, and the mass of the electrode weighed in the air after immersion is m2. The radius r and height h of the electrode are measured, and the water density is ρ. Finally, the formula is used to calculate The porosity is obtained. The two electrodes are analyzed using electrochemical principles, and the actual surface area of the electrode is calculated by the electrochemical adsorption amount. The ratio of the actual surface area to the apparent surface area is the specific surface area. The experimental results are as follows: Figure 3 The specific surface area of the electrode prepared in Example 2 is 25.52 m 2 / cm 2 The porosity is 20.68%; the specific surface area of the electrode prepared in Example 3 is 20.37m 2 / cm 2 , the porosity is 17.33%.
[0064] 2. The electrode prepared by rapid sintering and the electrode prepared by ordinary sintering in Example 2 were immersed in a 3% mass concentration NaCl solution, and the electrodes were subjected to range test and electrochemical noise test using an electrochemical workstation. The experimental results are as follows: Figure 4 The electrode prepared in Example 2 has a range of 0.052 mV and an electrochemical noise of 3.15 nV; the electrode prepared in Example 3 has a range of 0.067 mV and an electrochemical noise of 4.33 nV.
[0065] It can be seen that the Ag / AgCl electrode obtained by the method of the present invention is mainly prepared from silver chloride powder, ultrafine silver powder and graphene as raw materials, and the preparation process is simple and easy to operate. The present invention increases the specific surface area and porosity of the electrode, and prepares the Ag / AgCl electrode by rapid sintering, thereby shortening the preparation time while ensuring excellent electrochemical performance, and the precise temperature control and uniform heating of rapid sintering are suitable for large-scale production.
[0066] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an all-solid-state Ag / AgCl electrode, characterized in that: The following steps are involved: (1) Grind silver chloride into a fine powder in a dark environment; (2) mixing silver chloride powder and ultrafine silver powder, adding graphene thereto, and then ball milling the mixed powder; (3) After the ball milling is completed, the mixture is filtered out and then dried; (4) In a dark environment, take the dried powder, sieve it, pour it into a tableting mold, and perform preliminary pressing into shape; (5) Compressing the preliminarily compressed sample more tightly by a tablet press; (6) placing the sample in a Joule heating device for rapid sintering; (7) After the fired electrode is polished, a wire is connected to the outside, and after packaging, it is placed in an acid solution for activation to obtain a graphene-doped all-solid-state Ag / AgCl electrode.
2. The preparation method according to claim 1, characterized in that: In step (1), the agglomerated silver chloride is ground into fine powder, the grinding time is 0.2-0.4h, and the whole process is performed in a dark environment.
3. The preparation method according to claim 1, characterized in that: The molar ratio of the silver chloride powder to the ultrafine silver powder in step (2) is 1:1, and graphene is added thereto to obtain a mixed powder with a graphene mass percentage of 3-5%; the mixed powder is placed in a ball mill, and anhydrous ethanol and agate beads of the same mass as the mixed powder are added; finally, the ball mill is placed in a planetary ball mill to ball mill the mixture, the ball milling speed is 300-500 r / min, and the ball milling time is 4-6 hours.
4. The preparation method according to claim 1, characterized in that: The drying temperature in step (3) is 50-80°C and the drying time is 8h.
5. The preparation method according to claim 1, characterized in that: In step (4), the amount of powder filled in each tableting step is 0.25-0.35 g.
6. The preparation method according to claim 1, characterized in that: In step (5), the tablet press applies a pressure of 200-230 MPa to the powder, and the pressure holding time is 10-15 min.
7. The preparation method according to claim 1, characterized in that: The Joule heating device in step (6) is set at a temperature of 350-450° C. and a sintering time of 15-25 seconds.
8. The preparation method according to claim 7, characterized in that: The Joule heating device in step (6) is set at a temperature of 400° C. and a sintering time of 15 s.
9. An all-solid-state Ag / AgCl electrode prepared by the method according to any one of claims 1 to 8.