Electrochromic electrolyte as well as preparation method and application thereof

By integrating the electrochromic layer, electrolyte layer and ion storage layer into one layer, using specific components and processes, the high cost and long response time of electrochromic devices are solved, and breakthroughs in stability and large-area manufacturing are achieved .

CN118915360APending Publication Date: 2024-11-08MYS GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411253938.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing electrochromic devices have high production cost, long color change response time, and are difficult to achieve large-area manufacturing, which limits their practical applications.

Method used

Integrate the electrochromic layer, electrolyte layer and ion storage layer in traditional electrochromic devices into one layer, using plasticizers, polymeric monomers, additives, sodium polystyrene sulfonate, and poly(3,4-ethylene). Electrochromic electrolytes of components such as dioxythiophene) and lithium salts simplify the production process through screen printing.

Benefits of technology

It reduces production costs, improves the stability and discoloration response speed of electrochromic devices, extends the service life of the device, and achieves large-area manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915360A_ABST
    Figure CN118915360A_ABST
Patent Text Reader

Abstract

The invention provides an electrochromic electrolyte as well as a preparation method and application thereof. The electrochromic electrolyte is prepared from a component A and a component B, the component A comprises a plasticizer, a polymeric monomer and an auxiliary agent; and the component B comprises sodium polystyrenesulfonate, poly (3, 4-ethylenedioxythiophene) and a lithium salt. According to the electrochromic electrolyte provided by the invention, an electrochromic layer, an electrolyte layer and an ion storage layer in a traditional electrochromic device are integrated into one layer, and the electrochromic device can be assembled in a silk-screen printing manner, so that the device structure is simplified, the cost is low, and the stability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrochromic devices, and in particular relates to an electrochromic electrolyte and a preparation method and application thereof. Background Art

[0002] Conventional electrochromic devices are usually composed of a multilayer structure of a transparent conductive electrode layer, an electrochromic layer, an electrolyte layer, an ion storage layer (or a second electrochromic layer), and a transparent conductive electrode layer, but their preparation process is complicated.

[0003] In recent years, with the continuous optimization and upgrading of the structure of electrochromic devices, an electrochromic device with a transparent conductive electrode layer, an electrochromic layer, an electrolyte layer, and a transparent conductive electrode layer structure can be obtained by adjusting the electrochromic material and the electrolyte layer. Compared with the traditional structure, the electrochromic device of this structure simplifies the preparation process of the device to a certain extent. CN112327555A discloses an electrochromic device and its preparation method and application in a smart window, wherein the electrochromic device includes an anode transparent conductive substrate and a cathode transparent conductive substrate arranged relatively, and an electrochromic layer and an electrolyte layer arranged between the anode transparent conductive substrate and the cathode transparent conductive substrate, wherein the anode transparent conductive substrate and the cathode transparent conductive substrate do not include an ion storage layer; the electrolyte layer is obtained by dripping a solution containing metal ions on the electrochromic layer, wherein the metal ions are metal cations with an oxidizing effect, and the solvent of the solution containing metal ions is one or more of acetonitrile, methanol, and ethanol, and the concentration of the solution containing metal ions is 0.01 to 0.5M. The electrochromic device provided by this technical solution combines the functions of the electrolyte layer and the ion storage layer in the traditional electrochromic device into one, so that it has both oxidation and ion transmission functions, thus simplifying the structure.

[0004] CN117406507A discloses a gel-based electrochromic device and a preparation method thereof, wherein the gel-based electrochromic device comprises a first transparent electrode layer, an electrochromic layer, a gel electrolyte layer and a second transparent electrode layer stacked in sequence; the gel electrolyte layer is a solvent of at least one of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, methyl ethyl carbonate and ethylene glycol dimethyl ether, and a cationic salt is a solute, and an organic gel electrolyte layer is formed by the reaction of functional groups between amino monomers and epoxy monomers; the average functionality of the reaction between the amino monomers and epoxy monomers is greater than 2. The gel-based electrochromic device provided by the technical solution not only has excellent electrochromic performance, but also avoids safety hazards such as leakage, and has the advantages of safety and stability.

[0005] However, most of the electrochromic devices in the prior art still have problems such as high manufacturing cost, long color change response time, and difficulty in large-scale manufacturing, which greatly restricts their practical applications.

[0006] Therefore, it is necessary to develop an electrochromic device with low manufacturing cost, short color change response time and good stability. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention aims to provide an electrochromic electrolyte and its preparation method and application. The electrochromic electrolyte integrates the electrochromic layer, electrolyte layer and ion storage layer in the traditional electrochromic device into one layer, which simplifies the device structure, has low cost and good stability.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides an electrochromic electrolyte, wherein the raw materials for preparing the electrochromic electrolyte include component A and component B; the component A includes a plasticizer, a polymerization monomer and an auxiliary agent; the component B includes sodium polystyrene sulfonate (PSS), poly(3,4-ethylenedioxythiophene) (PEDOT) and a lithium salt.

[0010] Preferably, the plasticizer includes any one of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate or an ionic liquid, or a combination of at least two thereof.

[0011] Preferably, the polymerizable monomer includes any one of acryloylmorpholine, ethoxyethoxyethyl acrylate, tetrahydrofuran acrylate or methyl methacrylate, or a combination of at least two thereof.

[0012] Preferably, the mass ratio of the plasticizer to the polymerizable monomer is (2-3):1, for example, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1 or 2.9:1, etc.

[0013] Preferably, the auxiliary agent includes a thickener and a photoinitiator.

[0014] Preferably, the thickener comprises polycarbonate diol and / or polyvinyl pyrrolidone.

[0015] Preferably, the photoinitiator includes photoinitiator 184 and / or photoinitiator TPO.

[0016] Preferably, based on 100% of the total mass of component A, the mass of the thickener is 5% to 15%, for example, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13% or 14%.

[0017] Preferably, based on 100% of the total mass of component A, the mass of the photoinitiator is 0.1% to 1%, for example, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8% or 0.9%.

[0018] Preferably, the lithium salt includes any one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate or lithium hexafluorophosphate, or a combination of at least two thereof.

[0019] Preferably, the mass ratio of the sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is 5:(3-6):(0.5-2), for example, 5:4:0.8, 5:4:1.1, 5:4:1.4, 5:4:1.7, 5:5:0.8, 5:5:1.1, 5:5:1.4 or 5:5:1.7, and more preferably 5:(4-5):(1.5-2).

[0020] In the present invention, the mass ratio of sodium styrene sulfonate, poly (3,4-ethylenedioxythiophene) and lithium salt is preferably 5: (3-6): (0.5-2), and the electrochromic electrolyte has better flexibility, mechanical properties and electrochromism. If the content of sodium polystyrene sulfonate and poly (3,4-ethylenedioxythiophene) is too high, the electrochromic electrolyte will be too rigid, affecting the flexibility and mechanical properties of the electrochromic electrolyte; at the same time, it may cause the ion transmission channel to be blocked, the electrolyte ion conductivity to decrease, and affect the electrochromic effect. If the lithium salt content is low, the ion concentration in the electrochromic electrolyte is insufficient, which will reduce the ion conductivity, thereby reducing the response speed and color change effect of the electrochromic reaction; on the contrary, if its content is too high, the electrolyte ion concentration will be too high, causing ion aggregation, reducing ion mobility, and thus affecting the electrochromic effect.

[0021] Preferably, the mass ratio of component A to component B is 1:3 to 3:1, for example, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1, 2:1 or 2.5:1, and more preferably 1:1 to 2:1.

[0022] In the present invention, the electrochromic performance and mechanical properties of the electrochromic electrolyte are preferably good when the mass ratio of the A component to the B component is preferably 1:3 to 3:1. If the mass of the A component is too high, the viscosity of the electrochromic electrolyte may increase, the mobility of the ions may be reduced, and the ionic conductivity of the electrochromic electrolyte may be reduced, thereby affecting the electrochromic performance; if the mass of the A component is too low, a continuous polymer network may not be formed, affecting the mechanical and electrochemical properties of the electrochromic electrolyte.

[0023] In a second aspect, the present invention provides a method for preparing the electrochromic electrolyte as described in the first aspect, the preparation method comprising the following steps: mixing a plasticizer, a polymerization monomer, an additive, sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and a lithium salt, and curing to obtain the electrochromic electrolyte.

[0024] In a third aspect, the present invention provides an electrochromic device, comprising an upper substrate layer, an electrochromic electrolyte layer and a lower substrate layer stacked in sequence, wherein the electrochromic electrolyte layer comprises the electrochromic electrolyte as described in the first aspect.

[0025] In the present invention, the electrochromic electrolyte integrates the traditional electrochromic layer, electrolyte layer and ion storage layer into one layer, which effectively simplifies the structure of the electrochromic device, reduces the number of components, and thus reduces costs. The integrated design of the electrochromic device helps to improve the stability of the material during the electrochromic process, reduce the possibility of interface failure, and extend the service life of the device.

[0026] Preferably, the upper substrate layer and the lower substrate layer independently include any one of an ITO film, a metal grid or a PET film.

[0027] In a fourth aspect, the present invention provides a method for preparing the electrochromic device according to the third aspect, the preparation method comprising the following steps:

[0028] (1) mixing a plasticizer, a polymerization monomer, an additive, sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and a lithium salt to obtain an electrochromic electrolyte stock solution;

[0029] (2) Printing the electrochromic electrolyte stock solution obtained in step (1) on the surface of the upper substrate layer, curing it, and compounding it with the lower substrate layer to obtain the electrochromic device.

[0030] In the present invention, the electrochromic electrolyte in the electrochromic device is assembled by screen printing process, without the need to use expensive equipment, thus saving production costs to a great extent.

[0031] Preferably, the mixing in step (1) specifically comprises first mixing the plasticizer, the polymerizable monomer and the auxiliary agent to obtain component A, and then secondly mixing with sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt.

[0032] Preferably, the printing in step (2) comprises screen printing.

[0033] Preferably, the screen printing uses a screen mesh number of 200-300 meshes, such as 200 meshes, 250 meshes, or 300 meshes.

[0034] Preferably, the curing in step (2) comprises ultraviolet light curing.

[0035] Preferably, the curing time in step (2) is 10 to 30 seconds, for example, 12 seconds, 14 seconds, 16 seconds, 18 seconds, 20 seconds, 22 seconds, 24 seconds, 26 seconds or 28 seconds.

[0036] Preferably, the compounding in step (2) comprises hot pressing compounding.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The electrochromic device made of the electrochromic electrolyte of the present invention integrates the electrochromic layer, the electrolyte layer and the ion storage layer into one layer, which effectively simplifies the structure of the electrochromic device, reduces the number of components, and thus reduces the cost. The integrated design of the electrochromic device helps to improve the stability of the material during the electrochromic process, reduce the possibility of interface failure, and extend the service life of the device. The color change response time of the electrochromic device is 3 to 30 seconds, and the number of cycles is >2500 times. Preferably, the color change response time is 3 to 5 seconds, and the number of cycles is >3000 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A schematic diagram of the structure of the electrochromic device provided in Example 1;

[0040] Among them, 1-upper substrate layer; 2-electrochromic electrolyte layer; 3-lower substrate layer. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0042] The sources of some components in the examples are as follows:

[0043] Polycarbonate diol: Product number is P301655, manufacturer is Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0044] Polyvinylpyrrolidone: product number is P875214, manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd.;

[0045] Sodium polystyrene sulfonate: Product number is P821790, manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd.;

[0046] Poly(3,4-ethylenedioxythiophene): The product number is J0230, and the manufacturer is Suzhou Yaco Technology Co., Ltd.

[0047] Example 1

[0048] This embodiment provides an electrochromic device and a method for preparing the same. Figure 1 As shown, the electrochromic device comprises an upper substrate layer 1, an electrochromic electrolyte layer 2 and a lower substrate layer 3 which are stacked in sequence.

[0049] The upper substrate layer 1 is an ITO film with a thickness of 0.125 mm;

[0050] The electrochromic electrolyte layer 2 is an electrochromic electrolyte with a thickness of 120 μm, and the raw materials for preparing the electrochromic electrolyte include component A and component B; the component A is composed of a plasticizer (propylene carbonate), a polymer monomer (acryloyl morpholine), a thickener (polyvinyl pyrrolidone) and a photoinitiator (photoinitiator 184); the component B is composed of sodium polystyrene sulfonate, poly (3,4-ethylenedioxythiophene) and a lithium salt (lithium bistrifluoromethanesulfonyl imide);

[0051] The mass ratio of the plasticizer to the polymerizable monomer is 2:1;

[0052] Based on the total mass of component A being 100%, the mass of the thickener is 15%;

[0053] Based on the total mass of component A being 100%, the mass of the photoinitiator is 0.3%;

[0054] The mass ratio of the sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is 5:3:0.5;

[0055] The mass ratio of component A to component B is 1:3;

[0056] The lower substrate layer 3 is an ITO film with a thickness of 0.125 mm.

[0057] The preparation method comprises the following steps:

[0058] (1) mixing a plasticizer and a polymerizable monomer and stirring, adding a thickener and a photoinitiator during the stirring process to obtain a component A, then sequentially adding sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and a lithium salt to the component A, and ultrasonically dispersing the mixture until the mixture is uniform, to obtain an electrochromic electrolyte stock solution;

[0059] (2) The electrochromic electrolyte stock solution obtained in step (1) is screen-printed on the upper substrate layer, the screen printing is performed using a 250-mesh screen, UV-cured for 20 seconds, and then laminated with the lower substrate layer and hot-pressed at 100° C. for 2 minutes to obtain the electrochromic device.

[0060] Example 2

[0061] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:4:0.5; the mass ratio of component A to component B is adjusted to 1:2, and other conditions are the same as those in Embodiment 1.

[0062] Example 3

[0063] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:3:1; the mass ratio of component A to component B is adjusted to 2:3, and other conditions are the same as those in Embodiment 1.

[0064] Example 4

[0065] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:4:1; the mass ratio of component A and component B is adjusted to 2:3, and other conditions are the same as those in Embodiment 1.

[0066] Example 5

[0067] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:4:1.5; the mass ratio of component A to component B is adjusted to 2:1, and other conditions are the same as those in Embodiment 1.

[0068] Example 6

[0069] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:5:1.5; the mass ratio of component A to component B is adjusted to 2:1, and other conditions are the same as those in Embodiment 1.

[0070] Example 7

[0071] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:4:2; the mass ratio of component A and component B is adjusted to 1:1, and other conditions are the same as those in Embodiment 1.

[0072] Example 8

[0073] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:5:2; the mass ratio of component A and component B is adjusted to 1:1, and other conditions are the same as those in Embodiment 1.

[0074] Example 9

[0075] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:5:0.5; the mass ratio of component A to component B is adjusted to 3:1, and other conditions are the same as those in Embodiment 1.

[0076] Example 10

[0077] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:6:0.5; the mass ratio of component A to component B is adjusted to 3:1, and other conditions are the same as those in Embodiment 1.

[0078] Embodiment 11

[0079] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that component A is composed of a plasticizer (propylene carbonate), a polymerizable monomer (methyl methacrylate), a thickener (polycarbonate diol) and a photoinitiator (photoinitiator 184); component B is composed of sodium polystyrene sulfonate, poly (3,4-ethylenedioxythiophene) and a lithium salt (lithium bistrifluoromethanesulfonyl imide);

[0080] The mass ratio of plasticizer to polymerized monomer is 2:1;

[0081] Based on the total mass of component A being 100%, the mass of the thickener is 5%;

[0082] Based on the total mass of component A being 100%, the mass of the photoinitiator is 0.1%;

[0083] Other conditions are the same as in Example 1.

[0084] Example 12

[0085] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that component A is composed of a plasticizer (dimethyl carbonate), a polymerizable monomer (ethoxyethoxyethyl acrylate), a thickener (polyvinyl pyrrolidone) and a photoinitiator (photoinitiator TPO); component B is composed of sodium polystyrene sulfonate, poly (3,4-ethylenedioxythiophene) and a lithium salt (lithium bistrifluoromethanesulfonyl imide);

[0086] The mass ratio of plasticizer to polymerized monomer is 3:1;

[0087] Based on the total mass of component A being 100%, the mass of the thickener is 15%;

[0088] Based on the total mass of component A being 100%, the mass of the photoinitiator is 1%;

[0089] Other conditions are the same as in Example 1.

[0090] Embodiment 13

[0091] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the lithium salt (lithium bistrifluoromethanesulfonyl imide) is replaced with a lithium salt (lithium bisfluorosulfonyl imide) of the same mass.

[0092] Embodiment 14

[0093] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the lithium salt (lithium bistrifluoromethanesulfonyl imide) is replaced with a lithium salt (lithium trifluoromethanesulfonate) of the same mass.

[0094] Embodiment 15

[0095] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the lithium salt (lithium bistrifluoromethanesulfonyl imide) is replaced with a lithium salt (lithium hexafluorophosphate) of the same mass.

[0096] Example 16

[0097] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:3:0.3, and other conditions are the same as those in Embodiment 1.

[0098] Embodiment 17

[0099] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is 5:3:2.5, and other conditions are the same as Embodiment 1.

[0100] Embodiment 18

[0101] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the mass ratio of component A to component B is adjusted to 7:2, and other conditions are the same as those in Embodiment 1.

[0102] Embodiment 19

[0103] This embodiment provides an electrochromic device and a preparation method thereof, which is different from Embodiment 1 only in that the mass ratio of component A to component B is adjusted to 1:4, and other conditions are the same as those in Embodiment 1.

[0104] Embodiment 20

[0105] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:4:0.3; the mass ratio of component A to component B is adjusted to 5:1, and other conditions are the same as those in Embodiment 1.

[0106] Embodiment 21

[0107] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:3:0.3; the mass ratio of component A to component B is adjusted to 7:2, and other conditions are the same as those in Embodiment 1.

[0108] Embodiment 22

[0109] This embodiment provides an electrochromic device and a preparation method thereof, which differs from Embodiment 1 only in that the mass ratio of sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is adjusted to 5:2:0.1; the mass ratio of component A to component B is adjusted to 1:6, and other conditions are the same as those in Embodiment 1.

[0110] The electrochromic device provided in the above embodiment is tested, and the specific test method is as follows:

[0111] Response time: Take the electrochromic device provided in the above embodiment as the test object, turn on the power, set the color change voltage to 1.2V, and the fading voltage to 0.6V; the two flat-mouth clamps at the output end of the power supply are respectively clamped to the cathode and anode of the electrochromic device, and the negative electrode (black) is connected to the cathode of the electrochromic device, and the positive electrode (red) is connected to the anode of the electrochromic device; preset the color change and fading time, and observe the color change and fading state of the electrochromic film, and record the actual time of color change and fading. The actual time of color change and fading is the color change response time and the fading response time.

[0112] Number of cycles: The electrochromic device provided in the above embodiment is used as the test object, the power is turned on, the color change voltage is set to 1.2V, and the fading voltage is set to 0.6V; the two flat-mouth clamps at the output end of the power supply are respectively clamped to the cathode and anode of the electrochromic device, and the negative electrode (black) is connected to the cathode of the electrochromic device, and the positive electrode (red) is connected to the anode of the electrochromic device; the number of cycles is set to 3000 times, and the color change and fading states of the electrochromic film are observed. If the color change and fading states after 3000 cycles are not significantly changed from the initial state, it is recorded as the number of cycles>3000 times; if the color change and fading states after 3000 cycles are significantly changed from the initial state, but the color change and fading states after 2500 cycles are not significantly changed from the initial state, it is recorded as the number of cycles>2500 times.

[0113] The test results are shown in Table 1 below.

[0114] Table 1

[0115]

[0116]

[0117] According to the test results in Table 1, the color change response time of the electrochromic device provided in Examples 1-22 is 3 to 30 seconds, and the number of cycles is >2500 times.

[0118] Compared with Example 1, if the content of lithium salt in the mass ratio of sodium styrene sulfonate, poly (3,4-ethylenedioxythiophene) and lithium salt is too low (Example 16), the ion concentration is insufficient, which will reduce the ion conductivity, thereby reducing the response speed and color change effect of the electrochromic reaction; if the content of lithium salt in the mass ratio of sodium styrene sulfonate, poly (3,4-ethylenedioxythiophene) and lithium salt is too high (Example 17), it may cause the electrochromic electrolyte ion concentration to be too high, causing ion aggregation, reducing ion mobility, and thus affecting the electrochromic effect. It can be seen that the electrochromic device obtained by controlling the mass ratio of sodium styrene sulfonate, poly (3,4-ethylenedioxythiophene) and lithium salt to be 5: (3-6): (0.5-2) has better performance.

[0119] Compared with Example 1, if the mass ratio of component A to component B is too large (Example 18), the viscosity of the electrolyte may increase, the mobility of ions may be reduced, and the ionic conductivity of the electrochromic electrolyte may be reduced, affecting the electrochromic performance; if the mass ratio of component A to component B is too small (Example 19), a continuous polymer network may not be formed, affecting the mechanical and electrochemical properties of the electrochromic electrolyte. It can be seen that the electrochromic device obtained by controlling the mass ratio of component A to component B to be 1:3 to 3:1 has better performance.

[0120] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An electrochromic electrolyte, characterized in that: The raw materials for preparing the electrochromic electrolyte include component A and component B; the component A includes a plasticizer, a polymer monomer and an auxiliary agent; the component B includes sodium polystyrene sulfonate, poly (3,4-ethylenedioxythiophene) and a lithium salt.

2. The electrochromic electrolyte according to claim 1, characterized in that The plasticizer includes any one of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate or ionic liquid, or a combination of at least two thereof.

3. The electrochromic electrolyte according to claim 1 or 2, characterized in that: The polymerizable monomer includes any one or a combination of at least two of acryloylmorpholine, ethoxyethoxyethyl acrylate, tetrahydrofuran acrylate or methyl methacrylate; Preferably, the mass ratio of the plasticizer to the polymerizable monomer is (2-3):

1.

4. The electrochromic electrolyte according to any one of claims 1 to 3, characterized in that: The auxiliary agent includes a thickener and a photoinitiator; Preferably, the thickener comprises polycarbonate diol and / or polyvinyl pyrrolidone; Preferably, based on the total mass of component A being 100%, the mass of the thickener is 5% to 15%; Preferably, based on 100% of the total mass of component A, the mass of the photoinitiator is 0.1% to 1%.

5. The electrochromic electrolyte according to any one of claims 1 to 4, characterized in that: The lithium salt includes any one of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium trifluoromethanesulfonate or lithium hexafluorophosphate, or a combination of at least two thereof; Preferably, the mass ratio of the sodium styrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt is 5:(3-6):(0.5-2); Preferably, the mass ratio of component A to component B is 1:3 to 3:

1.

6. A method for preparing an electrochromic electrolyte according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: mixing a plasticizer, a polymerizable monomer, an auxiliary agent, sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and a lithium salt, and solidifying the mixture to obtain the electrochromic electrolyte.

7. An electrochromic device, characterized in that: The electrochromic device comprises an upper substrate layer, an electrochromic electrolyte layer and a lower substrate layer which are stacked in sequence, and the electrochromic electrolyte layer comprises the electrochromic electrolyte according to any one of claims 1 to 5.

8. The electrochromic device according to claim 7, characterized in that: The upper substrate layer and the lower substrate layer independently include any one of an ITO film, a metal mesh or a PET film.

9. A method for preparing an electrochromic device according to claim 7 or 8, characterized in that: The preparation method comprises the following steps: (1) mixing a plasticizer, a polymerization monomer, an additive, sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and a lithium salt to obtain an electrochromic electrolyte stock solution; (2) Printing the electrochromic electrolyte stock solution obtained in step (1) on the surface of the upper substrate layer, curing it, and compounding it with the lower substrate layer to obtain the electrochromic device.

10. The preparation method according to claim 9, characterized in that: The mixing in step (1) specifically comprises first mixing the plasticizer, the polymerizable monomer and the auxiliary agent to obtain component A, and then secondly mixing with sodium polystyrene sulfonate, poly(3,4-ethylenedioxythiophene) and lithium salt; Preferably, the printing in step (2) comprises screen printing; Preferably, the screen printing adopts a screen mesh number of 200 to 300 meshes; Preferably, the curing in step (2) comprises ultraviolet light curing; Preferably, the curing time in step (2) is 10 to 30 seconds; Preferably, the compounding in step (2) comprises hot pressing compounding.