Composite soft magnetic material and preparation method and application thereof
By forming a composite inorganic insulating layer and rare earth oxide layer on the core surface of the soft magnetic material, combined with magnetron sputtering technology, the problems of degradation of insulation performance and permeability attenuation of soft magnetic materials under high pressure are solved, achieving low loss and high The effect of resistivity is suitable for large-scale production.
Patent Information
- Application Number
- CN202411113976.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
AI Technical Summary
The insulating film of existing soft magnetic materials is easily fragile when formed under high pressure, resulting in degradation of insulation performance and improvement of high-frequency performance and losses. The traditional preparation method is complex, time-consuming and unfavorable to the environment, and the problem of permeability attenuation is difficult. solve.
The composite inorganic insulating layer, rare earth oxide layer and ferrite insulating layer are prepared on the surface of the soft magnetic core. A dense and uniform inorganic insulating layer is generated by high-temperature nitriding and oxidation treatment, and a rare earth oxide and iron are formed through magnetron sputtering technology. The oxygen insulating layer works synergistically to improve resistivity and compressive resistance, reduce loss and permeability attenuation.
It is realized that the insulating layer is not easy to break and fall off under high voltage, reduces losses, improves magnetic permeability and resistivity, simplifies the preparation process, is suitable for large-scale production, and maintains good performance at high frequency.
Smart Images

Figure BDA0004993109250000151 
Figure BDA0004993109250000161
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetic materials and relates to a composite soft magnetic material and a preparation method and application thereof. Background Art
[0002] With the development of electronic power technology, it is an inevitable trend for electronic devices to develop in the direction of miniaturization, high frequency and high current. In the future, higher requirements will be placed on the performance indicators of soft magnetic materials. Common metal magnetic powder core materials include iron-nickel, iron-silicon, iron-silicon-aluminum, iron-nickel-molybdenum, etc. Among them, iron-nickel has the highest DC bias performance, high saturation magnetic induction intensity and low loss, so it has a large market.
[0003] In traditional insulation coating, liquid phase coating method (such as precipitation method, sol-gel method, microemulsion method, etc.) and phosphoric acid passivation to generate phosphate and other methods of coating inorganic insulating materials are used. They have the characteristics of uniform integrity, controllable thickness, high resistivity of the coating material, and good thermal stability.
[0004] CN109461558A discloses a low-loss FeSiAl magnetic powder core composite coating method. The composite coating method includes powder selection, phosphoric acid coating, MnZn ferrite coating, pressing, annealing, and spraying. The process is low in cost and simple to operate, greatly improving the powder coating effect. The phosphoric acid-MnZn ferrite composite coating process can avoid the use of non-magnetic coating agents to cause the saturation magnetization and magnetic permeability of the magnetic powder core to decrease. Under the condition of ensuring high magnetic permeability, low-loss high-performance FeSiAl magnetic powder cores can be prepared. However, this method has disadvantages, such as the magnetic powder is formed under high pressure, and its insulating film is easily broken, resulting in a decrease in insulation performance; the magnetic powder insulating film generally undergoes thermal decomposition above 600°C, which reduces insulation performance, reduces high-frequency performance, and increases losses.
[0005] CN109979701A discloses a double-layer inorganic insulating coated soft magnetic powder and a preparation method thereof. The double-layer inorganic insulating coated soft magnetic powder comprises magnetic powder and a transition oxide layer and a dense oxide layer sequentially coated on the outer surface of the magnetic powder from the inside to the outside. The transition oxide layer is formed by in-situ oxidation on the surface of the magnetic powder, so that the transition oxide layer not only has a high bonding strength between the magnetic powder and the transition oxide layer, but also has good chemical wettability and high bonding strength at the interface between the transition oxide layer and the dense oxide layer. However, the dense oxide layer in the patent is prepared by a chemical deposition method, but the entire preparation process is relatively complicated, with many influencing factors, which is not conducive to controlling product uniformity, is time-consuming, and has low production efficiency. At the same time, this method involves multi-step chemical reactions and metal solutions, which are easy to pollute the environment. And the excessive inorganic oxide insulation layer on the surface of the soft magnetic powder particles is prone to cause a large degree of attenuation of the magnetic permeability.
[0006] CN102136331A discloses a high-efficiency soft magnetic composite material and a preparation method thereof, wherein the soft magnetic metal and the soft magnetic ferrite powder are mixed uniformly in proportion, so that the soft magnetic ferrite powder is coated on the surface of the soft magnetic metal, and then the composite sintering is formed by discharge plasma sintering densification, and finally stress relief annealing heat treatment is performed. The soft magnetic composite material prepared in the patent has the characteristics of high saturation magnetic induction intensity and high resistivity, high magnetic permeability, low coercive force, low loss, and excellent comprehensive mechanical properties. However, the direct soft magnetic ferrite contact of the soft magnetic metal particles in the patent will cause the metal ions in the outer ferrite insulating layer and the core particles to undergo mutual diffusion, and the core Fe element will diffuse and activate, resulting in attenuation of the loss under high frequency. At the same time, the production environment required for the discharge plasma sintering equipment used in the patent is relatively high, which is not conducive to large-scale production.
[0007] The coating layer of the soft magnetic composite material obtained by the above scheme has insufficient density, reduced insulation performance under high voltage, poor interface bonding of the coating layer, and is easy to break and fall off during the pressing process, causing the insulation performance to decrease or even fail. Summary of the invention
[0008] The purpose of the present invention is to provide a composite soft magnetic material and a preparation method and application thereof. The present invention prepares a composite inorganic insulating layer, a rare earth oxide layer and a ferrite insulating layer on the surface of a soft magnetic core. The three act synergistically to reduce the problem of magnetic powder being easily broken and falling off during the pressing and molding process, causing the insulation performance to decline or even fail, while ensuring the magnetic permeability of the soft magnetic material.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a composite soft magnetic material, comprising a soft magnetic core and a composite inorganic insulating layer, a rare earth oxide layer and a ferrite insulating layer sequentially coated on the surface of the soft magnetic core.
[0011] The composite inorganic insulating layer in the composite soft magnetic material of the present invention is dense and uniform, has good interface bonding with the soft magnetic core particles, and has high resistivity. The rare earth oxide layer has excellent dielectric constant, high compressive resistance and high resistivity, thereby improving the overall resistance of the magnetic core, reducing losses, and can reduce problems such as cracking and detachment of the coating layer during pressing. The outermost ferrite insulating layer can compensate for the problem of magnetic permeability attenuation caused by multiple layers of inorganic insulation.
[0012] Preferably, the soft magnetic core comprises Sendust soft magnetic material.
[0013] Preferably, taking the mass of the sendust soft magnetic material as 100%, the mass fraction of silicon in the sendust soft magnetic material is 7.7-9.8%, not limited to the listed values, and other values not listed within the numerical range are also applicable, for example: 7.7%, 8%, 8.5%, 9% or 9.8%, etc. The mass fraction of aluminum is 5.2-6.6%, for example: 5.2%, 5.5%, 6%, 6.2% or 6.6%, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable, and the rest is iron.
[0014] Preferably, the median particle size D50 of the soft magnetic core is 55-65 μm, for example, 55 μm, 58 μm, 60 μm, 62 μm or 65 μm, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the composite inorganic insulating layer comprises aluminum nitride, aluminum oxide, silicon oxide and composite rare earth aluminum oxide.
[0016] Preferably, the mass ratio of the aluminum nitride, aluminum oxide, silicon oxide and composite rare earth aluminum oxide is 1:(4-5):(2-2.5):(6-7), for example: 1:4:2:6, 1:4.5:2.2:6.5, 1:4.2:2.2:7, 1:5:2:6 or 1:5:2.5:7, etc., not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0017] Preferably, the thickness of the composite inorganic insulating layer is 40-60 nm, for example, 40 nm, 45 nm, 50 nm, 55 nm or 60 nm, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] Preferably, the rare earth elements in the rare earth oxide layer and the composite rare earth alumina both include lanthanum.
[0019] The composite rare earth alumina in the composite inorganic insulating layer of the present invention is that during the preparation of the rare earth oxide layer, part of the rare earth will enter the gaps of the composite inorganic insulating layer and combine with alumina to form composite rare earth alumina, further improving the bonding strength between the rare earth oxide layer and the composite inorganic insulating layer.
[0020] Preferably, the thickness of the rare earth oxide layer is 20-40 nm, for example, 20 nm, 25 nm, 30 nm, 35 nm or 40 nm, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] Preferably, the material of the ferrite insulating layer includes manganese-zinc ferrite.
[0022] Preferably, the thickness of the ferrite insulating layer is 100-120 nm, for example, 100 nm, 105 nm, 110 nm, 115 nm or 120 nm, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] In a second aspect, the present invention provides a method for preparing the composite soft magnetic material as described in the first aspect, the preparation method comprising the following steps:
[0024] (1) After nitriding the soft magnetic core material, oxidation treatment is performed to obtain a soft magnetic material coated with a composite inorganic insulating layer;
[0025] (2) performing a first magnetron sputtering treatment on the soft magnetic material coated with the composite inorganic insulating layer obtained in step (1) using a rare earth oxide to obtain a precursor;
[0026] (3) Using a ferrite material, the precursor obtained in step (2) is subjected to a second magnetron sputtering treatment to obtain the composite soft magnetic material.
[0027] The present invention utilizes high-temperature nitridation and oxidation to generate an AlN / Al2O3 / SiO2 inorganic insulating layer on the surface of alloy powder particles. The inorganic insulating layer has dense and uniform film formation, good interface bonding with soft magnetic particles, and high resistivity. Then, a La2O5 insulating layer is sputtered by magnetron sputtering. The sputtered La2O5 can be partially filled into the AlN / Al2O3 / SiO2 inorganic insulating layer, and combined with Al2O3 on the soft magnetic powder particles to form La2O5-Al2O3 to improve the bonding strength between the two layers. The La2O5 film has excellent dielectric constant, high compressive strength and high resistivity, thereby improving the overall resistance of the magnetic core, reducing losses, and reducing the problems of coating layer rupture and separation during pressing. Finally, sputtering ferrite compensates for the problem of magnetic permeability attenuation caused by multi-layer inorganic insulation.
[0028] Preferably, the soft magnetic core material in step (1) comprises sendust soft magnetic alloy powder.
[0029] Preferably, the nitrogen flow rate of the nitridation treatment in step (1) is 200 to 500 mL / min, for example, 200 mL / min, 250 mL / min, 300 mL / min, 400 mL / min or 500 mL / min, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the pressure of the nitriding treatment in step (1) is 1 to 1.5 atm, for example, 1 atm, 1.1 atm, 1.2 atm, 1.3 atm, 1.4 atm or 1.5 atm, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the temperature of the nitriding treatment in step (1) is 900-1100°C, for example, 900°C, 950°C, 1000°C, 1050°C or 1100°C, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the time of the nitriding treatment in step (1) is 0.5 to 1.5 h, for example, 0.5 h, 0.8 h, 1 h, 1.2 h or 1.5 h, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the nitriding treatment in step (1) is followed by cooling treatment and then oxidation treatment.
[0034] Preferably, the oxygen flow rate of the oxidation treatment in step (1) is 100 to 300 mL / min, for example, 100 mL / min, 150 mL / min, 200 mL / min, 250 mL / min or 300 mL / min, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the pressure of the oxidation treatment in step (1) is 1 to 1.5 atm, for example, 1 atm, 1.1 atm, 1.2 atm, 1.3 atm, 1.4 atm or 1.5 atm, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] Preferably, the temperature of the oxidation treatment in step (1) is 400-500°C, for example, 400°C, 420°C, 450°C, 480°C or 500°C, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the oxidation treatment time in step (1) is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the rare earth oxide in step (2) comprises lanthanum oxide.
[0039] Preferably, the background vacuum degree of the first magnetron sputtering treatment in step (2) is 3×10 -5 Pa~6×10 -5 Pa, for example: 3×10 -5 Pa, 3.5×10 -5 Pa, 4×10 -5 Pa, 5×10-5 Pa or 6×10 -5 Pa, etc. are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] Preferably, the atmosphere of the first magnetron sputtering treatment in step (2) includes argon and oxygen.
[0041] Preferably, the flow ratio of argon to oxygen in step (2) is (1-5):1, for example: 1:1, 2:1, 3:1, 4:1 or 5:1, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, in step (2), the gas pressure of the first magnetron sputtering treatment is 0.5-0.8 Pa, for example, 0.5 Pa, 0.55 Pa, 0.6 Pa, 0.7 Pa or 0.8 Pa, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the power of the first magnetron sputtering treatment in step (2) is 100-140 W, for example: 100 W, 110 W, 120 W, 130 W or 140 W, etc., not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0044] Preferably, the time of the first magnetron sputtering treatment in step (2) is 0.5 to 2.5 h, for example: 0.5 h, 1 h, 1.5 h, 2 h or 2.5 h, etc., not limited to the listed values, other values not listed within the numerical range are also applicable.
[0045] Preferably, the ferrite material in step (3) includes manganese-zinc ferrite.
[0046] Preferably, the background vacuum degree of the second magnetron sputtering treatment in step (3) is 1×10 -3 Pa~5×10 -3 Pa, for example: 1×10 -3 Pa, 2×10 -3 Pa, 3×10 -3 Pa, 4×10 -3 Pa or 5×10 -3 Pa, etc. are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the atmosphere of the second magnetron sputtering treatment in step (3) includes argon.
[0048] Preferably, in step (3), the gas pressure of the second magnetron sputtering treatment is 0.8-1.2 atm, for example, 0.8 atm, 0.9 atm, 1 atm, 1.1 atm or 1.2 atm, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] Preferably, the sputtering power of the second magnetron sputtering treatment in step (3) is 150-250 W, for example, 150 W, 180 W, 200 W, 220 W or 250 W, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] Preferably, in step (3), the vibration power of the second magnetron sputtering treatment is 20 to 40 W, for example, 20 W, 25 W, 30 W, 35 W or 40 W, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0051] Preferably, the time of the second magnetron sputtering treatment in step (3) is 2 to 4 hours, for example: 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, etc., not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0052] In a third aspect, the present invention provides a composite magnetic powder core, wherein the composite magnetic powder core comprises the composite soft magnetic material as described in the first aspect.
[0053] The composite magnetic powder core of the present invention has the advantages of low power loss, good DC superposition performance and the insulation layer is not easy to break and fall off under high voltage.
[0054] In a fourth aspect, the present invention provides a method for preparing the composite magnetic powder core as described in the third aspect, the preparation method comprising the following steps:
[0055] The composite soft magnetic material is mixed with a binder, and then pressed and annealed to obtain the composite magnetic powder core.
[0056] Preferably, the binder includes any one of epoxy resin, phenolic resin or polyurethane resin or a combination of at least two thereof. Typical but non-limiting combinations include a combination of epoxy resin and polyurethane resin, a combination of epoxy resin and phenolic resin, or a combination of phenolic resin and polyurethane resin.
[0057] Preferably, the mass ratio of the binder to the composite soft magnetic material is (0.5-2.5):100, for example: 0.5:100, 1:100, 1.5:100, 2:100 or 2.5:100, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0058] In the process of preparing magnetic powder cores with the composite soft magnetic material of the present invention, the content of the binder needs to be controlled within the above range. If the amount of binder added is too high, the binder will decompose during high-temperature annealing, resulting in an increase in the voids inside the magnetic ring and deterioration of the magnetic properties.
[0059] Preferably, the pressing pressure is 20-25 T / cm 2 , for example: 20T / cm 2 , 21T / cm 2 , 22T / cm 2 , 24T / cm 2 or 25T / cm 2 The present invention is not limited to the numerical values listed, and other numerical values not listed within the numerical range are also applicable.
[0060] Preferably, the pressing time is 1 to 5 seconds, for example, 1 second, 2 seconds, 3 seconds, 4 seconds or 5 seconds, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0061] Preferably, the annealing temperature is 650-750°C, for example, 650°C, 680°C, 700°C, 720°C or 750°C, etc., and is not limited to the listed values, and other values not listed within the range are also applicable.
[0062] Preferably, the annealing treatment time is 0.5 to 1 h, for example, 0.5 h, 0.6 h, 0.8 h, 0.9 h or 1 h, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] (1) The present invention prepares a composite inorganic insulating layer, a rare earth oxide layer and a ferrite insulating layer on the surface of a soft magnetic core by high-temperature nitridation, oxidation and magnetron sputtering. The three layers work synergistically to ensure the magnetic permeability of the soft magnetic material while reducing the problem of magnetic powder being easily broken and falling off during the pressing process, which causes the insulation performance to deteriorate or even fail.
[0065] (2) The preparation method of the composite soft magnetic material of the present invention is simple, and the high-temperature nitridation and oxidation method and magnetron sputtering method adopted in the overall process are suitable for mass production and are environmentally friendly.
[0066] (3) The magnetic powder core prepared using the composite soft magnetic material of the present invention has the advantages of low power loss, good DC superposition performance and the insulation layer is not easy to crack and fall off under high voltage.
[0067] (4) The relative magnetic permeability of the magnetic powder core made of the composite soft magnetic material of the present invention can reach above 71.4, and the power loss can reach 794kW / m 3 Below 100Oe, the DC superposition characteristic can reach more than 59%. By adjusting the preparation conditions, the relative magnetic permeability of the magnetic powder core can reach more than 81.6, and the power loss can reach 716kW / m 3 Below, the DC superposition characteristic of 100Oe can reach more than 62%. It is proved that the Sendust composite magnetic powder core prepared by the present invention has lower power loss and good DC superposition characteristic. DETAILED DESCRIPTION
[0068] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0069] The sendust soft magnetic alloy powders used in the embodiments of the present invention and the comparative examples are all -100 to +325 mesh sendust soft magnetic alloy powders, and the chemical composition mass percentage of the soft magnetic alloy powders is: Si9.2%, Al6.1%, and the rest is Fe. Before preparation, the following treatments are performed:
[0070] The Sendust soft magnetic alloy powder was stirred and cleaned with acetone for 30 minutes, and then placed in an oven to dry at 80° C. The dried Sendust soft magnetic alloy powder was placed in a tube furnace and N2 was introduced for 30 minutes to ensure that there was no residual air inside the powder.
[0071] Example 1
[0072] This embodiment provides a composite soft magnetic material, the composite soft magnetic material comprising a sendust core with a median particle size D50 of 75 μm and a composite inorganic insulating layer with a thickness of 50 nm, a lanthanum oxide layer with a thickness of 30 nm and a manganese zinc ferrite insulating layer with a thickness of 110 nm sequentially coated on the surface of the sendust core, wherein the composite inorganic insulating layer comprises aluminum nitride, aluminum oxide, silicon oxide and composite rare earth aluminum oxide in a mass ratio of 1:4:2:6. The preparation method of the composite soft magnetic material is as follows:
[0073] (1) Raise the temperature of the tube furnace to 1000°C, the N2 flow rate is 350mL / min, the pressure of the N2 is 1atm, the high-temperature nitriding time is 1h, and N2 is still introduced during the cooling process. After cooling, O2 is introduced into the interior at a temperature of 450°C, an O2 flow rate of 150mL / min, the pressure of the O2 is 1atm, and the time is 30min. During the cooling process, N2 is introduced to obtain a soft magnetic material coated with a composite inorganic insulating layer;
[0074] (2) The soft magnetic material coated with the composite inorganic insulating layer is placed in the sputtering chamber of the powder magnetron sputtering apparatus, and the required La2O5 target material is installed on the magnetron sputtering target holder. The purity of the La2O5 target material is 99.9%. The sputtering chamber is closed and evacuated to a vacuum level of 4×10 -5 Pa. Argon and oxygen (the flow ratio of argon and oxygen is 4:1) are introduced into the sputtering chamber to make the internal pressure reach 0.6Pa. The sputtering power is adjusted to 120W, and sputtering is started at room temperature for 1h. After the sputtering is completed, the internal pressure of the sputtering chamber reaches 1atm, the sputtering chamber door is opened, and the sample is taken out to obtain the precursor;
[0075] (3) Place the precursor in the sputtering chamber of the powder magnetron sputtering instrument and install the manganese-zinc ferrite target on the magnetron sputtering target holder. Close the sputtering chamber and evacuate it so that the background vacuum of the sputtering chamber is 2×10 -3 Pa. Argon gas was introduced into the sputtering chamber to make the internal pressure reach 1 atm. The vibration power was adjusted to 30 W, the sputtering power was adjusted to 200 W, and sputtering was started for 3 hours. The sputtering chamber door was opened, and the powder particles were taken out to obtain the composite soft magnetic material.
[0076] Example 2
[0077] This embodiment provides a composite soft magnetic material, which includes a sendust core with a median particle size D50 of 60 μm and a composite inorganic insulating layer with a thickness of 40 nm, a lanthanum oxide layer with a thickness of 20 nm, and a manganese-zinc ferrite insulating layer with a thickness of 110 nm, which are sequentially coated on the surface of the sendust core, wherein the composite inorganic insulating layer includes aluminum nitride, aluminum oxide, silicon oxide, and composite rare earth aluminum oxide in a mass ratio of 1:4.5:2.2:6.5. The preparation method of the composite soft magnetic material is as follows:
[0078] (1) Raise the temperature of the tube furnace to 900°C, the N2 flow rate is 200mL / min, the pressure of the N2 is 1atm, the high-temperature nitriding time is 0.5h, and N2 is still introduced during the cooling process. After cooling, O2 is introduced into the interior at a temperature of 400°C, an O2 flow rate of 100mL / min, the pressure of the O2 is 1atm, and the time is 20min. During the cooling process, N2 is introduced instead to obtain a soft magnetic material coated with a composite inorganic insulating layer;
[0079] (2) The soft magnetic material coated with the composite inorganic insulating layer is placed in the sputtering chamber of the powder magnetron sputtering apparatus, and the required La2O5 target material is installed on the magnetron sputtering target holder. The purity of the La2O5 target material is 99.9%. The sputtering chamber is closed and evacuated to a vacuum level of 3×10 -5Pa. Argon and oxygen (the flow ratio of argon and oxygen is 5:1) are introduced into the sputtering chamber to make the internal pressure reach 0.5Pa. The sputtering power is adjusted to 100W, and sputtering is started at room temperature for 0.5h. After the sputtering is completed, the internal pressure of the sputtering chamber reaches 1atm, the sputtering chamber door is opened, and the sample is taken out to obtain the precursor;
[0080] (3) Place the precursor in the sputtering chamber of the powder magnetron sputtering instrument and install the manganese-zinc ferrite target on the magnetron sputtering target holder. Close the sputtering chamber and evacuate it so that the background vacuum of the sputtering chamber is 1×10 -3 Pa. Argon gas was introduced into the sputtering chamber to make the internal pressure reach 1 atm. The vibration power was adjusted to 20 W, the sputtering power was adjusted to 150 W, and sputtering was started for 2 h. The sputtering chamber door was opened, and the powder particles were taken out to obtain the composite soft magnetic material.
[0081] Example 3
[0082] This embodiment provides a composite soft magnetic material, which includes a sendust core with a median particle size D50 of 65 μm and a composite inorganic insulating layer with a thickness of 60 nm, a lanthanum oxide layer with a thickness of 40 nm and a manganese-zinc ferrite insulating layer with a thickness of 120 nm, which are sequentially coated on the surface of the sendust core, wherein the composite inorganic insulating layer includes aluminum nitride, aluminum oxide, silicon oxide and composite rare earth aluminum oxide in a mass ratio of 1:5:2.5:7. The preparation method of the composite soft magnetic material is as follows:
[0083] (1) Raise the temperature of the tube furnace to 1100°C, the N2 flow rate is 500mL / min, the pressure of the N2 is 1.5atm, the high-temperature nitriding time is 1.5h, and N2 is still introduced during the cooling process. After cooling, O2 is introduced into the interior at a temperature of 500°C, an O2 flow rate of 300mL / min, the pressure of the O2 is 1.5atm, and the time is 40min. During the cooling process, N2 is introduced to obtain a soft magnetic material coated with a composite inorganic insulating layer;
[0084] (2) The soft magnetic material coated with the composite inorganic insulating layer is placed in the sputtering chamber of the powder magnetron sputtering apparatus, and the required La2O5 target material is installed on the magnetron sputtering target holder. The purity of the La2O5 target material is 99.9%. The sputtering chamber is closed and evacuated to a vacuum level of 6×10 -5 Pa. Argon and oxygen (the flow ratio of argon and oxygen is 1:1) are introduced into the sputtering chamber to make the internal pressure reach 0.8Pa. The sputtering power is adjusted to 140W, and sputtering is started at room temperature for 2.5h. After the sputtering is completed, the internal pressure of the sputtering chamber reaches 1atm, the sputtering chamber door is opened, and the sample is taken out to obtain the precursor;
[0085] (3) Place the precursor in the sputtering chamber of the powder magnetron sputtering instrument and install the manganese-zinc ferrite target on the magnetron sputtering target holder. Close the sputtering chamber and evacuate it so that the background vacuum of the sputtering chamber is 5×10 -3 Pa. Argon gas was introduced into the sputtering chamber to make the internal pressure reach 1 atm. The vibration power was adjusted to 40 W, the sputtering power was adjusted to 250 W, and sputtering was started for 4 hours. The sputtering chamber door was opened, and the powder particles were taken out to obtain the composite soft magnetic material.
[0086] Example 4
[0087] The only difference between this embodiment and embodiment 1 is that the nitrogen flow rate of the nitridation treatment in step (1) is 800 mL / min, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0088] Example 5
[0089] The only difference between this embodiment and embodiment 1 is that the nitrogen flow rate of the nitridation treatment in step (1) is 100 mL / min, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0090] Example 6
[0091] The only difference between this embodiment and embodiment 1 is that the oxygen flow rate of the oxidation treatment in step (1) is 50 mL / min, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0092] Example 7
[0093] The only difference between this embodiment and embodiment 1 is that the oxygen flow rate of the oxidation treatment in step (1) is 400 mL / min, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0094] Example 8
[0095] The only difference between this embodiment and embodiment 1 is that the power of the magnetron sputtering treatment in step (2) is 80 W, the sputtering time is 0.3 h, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0096] Example 9
[0097] The only difference between this embodiment and embodiment 1 is that the power of the magnetron sputtering treatment in step (2) is 150 W, the sputtering time is 3 h, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0098] Example 10
[0099] The only difference between this embodiment and embodiment 1 is that the power of the magnetron sputtering treatment in step (3) is 100 W, the sputtering time is 1 hour, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0100] Embodiment 11
[0101] The only difference between this embodiment and embodiment 1 is that the power of the magnetron sputtering treatment in step (3) is 300 W, the sputtering time is 5 h, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0102] Comparative Example 1
[0103] The only difference between this comparative example and Example 1 is that no oxidation treatment is performed, and other conditions and parameters are exactly the same as those in Example 1.
[0104] Comparative Example 2
[0105] The only difference between this comparative example and Example 1 is that no nitriding treatment is performed, and other conditions and parameters are exactly the same as those in Example 1.
[0106] Comparative Example 3
[0107] The only difference between this comparative example and Example 1 is that step (2) is not performed, and the other conditions and parameters are exactly the same as those in Example 1.
[0108] Comparative Example 4
[0109] The only difference between this comparative example and Example 1 is that step (3) is not performed, and the other conditions and parameters are exactly the same as those in Example 1.
[0110] Performance Test:
[0111] The composite soft magnetic material obtained in the embodiment and the comparative example was mixed with 1.2% epoxy resin and granulated uniformly. The granulated powder was placed in a mold and heated at 21T / cm 2 The pressed magnetic ring with an outer diameter of 12.7 mm and an inner diameter of 7.7 mm was placed in a N2 atmosphere and annealed at 700°C for 1 hour to obtain a magnetic powder core, which was tested as follows:
[0112] (1) Magnetic permeability test: The magnetic ring is tested for the real part of magnetic permeability μ' at 100 kHz using an Agilent E4991A analyzer.
[0113] (2) Power loss test: The magnetic rings provided in Examples 1-11 and Comparative Examples 1-5 were uniformly wound with 30+5 turns of copper wire with a diameter of 0.4 mm. The test conditions were 100 kHz, 100 mT, and 25°C.
[0114] (3) DC superposition characteristics (100Oe) test: The magnetic rings provided in Examples 1-8 and Comparative Examples 1-5 were uniformly wound with 30 turns of copper wire with a diameter of 0.4 mm. The test conditions were 100kHz, 1V, and 25°C. The DC superposition performance of the magnetic rings under a magnetic field strength of 100Oe was calculated. The test results are shown in Table 1:
[0115] Table 1
[0116]
[0117]
[0118] As can be seen from Table 1, from Examples 1-11, the relative magnetic permeability of the magnetic powder core made of the composite soft magnetic material of the present invention can reach above 71.4, and the power loss can reach 794kW / m 3 Below 100Oe, the DC superposition characteristic can reach more than 59%. By adjusting the preparation conditions, the relative magnetic permeability of the magnetic powder core can reach more than 81.6, and the power loss can reach 716kW / m 3 Below, the 100Oe DC superposition characteristic can reach more than 62%, indicating that the Sendust Aluminum composite magnetic powder core prepared by the present invention has lower power loss and good DC superposition characteristic.
[0119] By comparing Example 1 with Example 4-5, it can be seen that during the preparation process of the composite soft magnetic material of the present invention, the nitrogen flow rate of the nitriding treatment will affect its performance. The nitrogen flow rate of the nitriding treatment is controlled at 200-500 mL / min, and the performance of the composite soft magnetic material is better. If the nitrogen flow rate of the nitriding treatment is too fast, the powder is excessively nitrided at high temperature, and the overall resistivity of the powder increases. Although the power loss and DC superposition characteristics are improved, the magnetic permeability is seriously attenuated. If the nitrogen flow rate of the nitriding treatment is too slow, the high-temperature nitriding is insufficient, the resistivity decreases, the power loss and DC superposition characteristics are affected, and the subsequent generation of aluminum oxide is affected, and the magnetic permeability is also attenuated.
[0120] By comparing Example 1 with Example 6-7, it can be seen that in the preparation process of the composite soft magnetic material of the present invention, the oxygen flow rate of the nitriding treatment will affect its performance. The oxygen flow rate of the nitriding treatment is controlled at 100-300 mL / min, and the performance of the composite soft magnetic material is better. If the oxygen flow rate of the nitriding treatment is too fast, the iron element in the powder is oxidized, so that the comprehensive performance is deteriorated. If the oxygen flow rate of the nitriding treatment is too slow, the powder generates insufficient amounts of aluminum oxide and silicon oxide, and the overall resistivity of the powder decreases. Although the magnetic permeability increases, the power loss and DC superposition characteristics are deteriorated.
[0121] By comparing Example 1 with Example 8-9, it can be seen that in the preparation process of the composite soft magnetic material of the present invention, the power and time of the magnetron sputtering treatment in step (2) will affect its performance. The power of the magnetron sputtering treatment in step (2) is controlled at 100-140W and the time is controlled at 0.5-2.5h, and the performance of the composite soft magnetic material is better. If the power of the magnetron sputtering treatment in step (2) is too large and the time is too long, the lanthanum oxide insulating layer is too thick, the overall resistivity of the powder increases, the magnetic permeability decreases, and the power loss and DC superposition characteristics are improved. If the power of the magnetron sputtering treatment in step (2) is too small and the time is too short, it is not enough to form the La2O5-Al2O3 composite film, and its excellent dielectric constant, high compressive strength and high resistivity characteristics cannot be fully utilized, resulting in serious deterioration of power loss and DC superposition characteristics.
[0122] By comparing Example 1 with Examples 10-11, it can be seen that in the preparation process of the composite soft magnetic material of the present invention, the power and time of the magnetron sputtering treatment in step (3) will affect its performance. The power of the magnetron sputtering treatment in step (3) is controlled at 150-250W and the time is controlled at 2-4h, and the performance of the composite soft magnetic material is better. If the power of the magnetron sputtering treatment in step (3) is too large and the time is too long, the resistivity of the powder as a whole decreases to a certain extent, so that the power loss and DC superposition characteristics are affected. If the power of the magnetron sputtering treatment in step (3) is too small and the time is too short, the magnetic permeability compensation caused by the introduction of ferrite is insufficient, so that the magnetic permeability decreases relatively.
[0123] By comparing Example 1 with Comparative Example 1, it can be seen that without oxidation treatment, the Al2O3 / SiO2 insulating layer does not appear on the powder surface, so that the overall resistivity of the magnetic powder core is low, the eddy current loss is increased, and the DC superposition characteristics are affected.
[0124] From the comparison between Example 1 and Comparative Example 2, it can be seen that without nitriding treatment, part of Fe is oxidized, resulting in a decrease in the magnetic permeability of the magnetic powder core. On the other hand, the hysteresis loss of the magnetic powder core increases due to the oxidation of Fe, resulting in an increase in the overall power loss.
[0125] From the comparison between Example 1 and Comparative Example 3, it can be seen that without the La2O5 insulating layer coating, the resistivity of the magnetic powder core is relatively reduced, which further affects the power loss and DC superposition characteristics.
[0126] From the comparison between Example 1 and Comparative Example 4, it can be seen that without the ferrite insulation layer coating, the magnetic permeability of the magnetic powder core is not compensated, resulting in a low magnetic permeability of the magnetic powder core.
[0127] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A composite soft magnetic material, characterized in that: The composite soft magnetic material comprises a soft magnetic core and a composite inorganic insulating layer, a rare earth oxide layer and a ferrite insulating layer which are sequentially coated on the surface of the soft magnetic core.
2. The composite soft magnetic material according to claim 1, characterized in that: The soft magnetic core comprises a sendust soft magnetic material; Preferably, based on the mass of the sendust soft magnetic material being 100%, the mass fraction of silicon in the sendust soft magnetic material is 7.7-9.8%, the mass fraction of aluminum is 5.2-6.6%, and the rest is iron; Preferably, the median particle size D50 of the soft magnetic core is 55-65 μm.
3. The composite soft magnetic material according to claim 1 or 2, characterized in that: The composite inorganic insulating layer comprises aluminum nitride, aluminum oxide, silicon oxide and composite rare earth aluminum oxide; Preferably, the mass ratio of the aluminum nitride, aluminum oxide, silicon oxide and composite rare earth aluminum oxide is 1:(4-5):(2-2.5):(6-7); Preferably, the thickness of the composite inorganic insulating layer is 40 to 60 nm; Preferably, the rare earth elements in the rare earth oxide layer and the composite rare earth alumina both include lanthanum; Preferably, the rare earth oxide layer has a thickness of 20-40 nm.
4. The composite soft magnetic material according to any one of claims 1 to 3, characterized in that: The material of the ferrite insulating layer includes manganese-zinc ferrite; Preferably, the thickness of the ferrite insulating layer is 100-120 nm.
5. A method for preparing the composite soft magnetic material according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) After nitriding the soft magnetic core material, oxidation treatment is performed to obtain a soft magnetic material coated with a composite inorganic insulating layer; (2) performing a first magnetron sputtering treatment on the soft magnetic material coated with the composite inorganic insulating layer obtained in step (1) using a rare earth oxide to obtain a precursor; (3) Using a ferrite material, the precursor obtained in step (2) is subjected to a second magnetron sputtering treatment to obtain the composite soft magnetic material.
6. The preparation method according to claim 5, characterized in that: The soft magnetic core material in step (1) comprises sendust soft magnetic alloy powder; Preferably, the nitrogen flow rate of the nitridation treatment in step (1) is 200 to 500 mL / min; Preferably, the pressure of the nitriding treatment in step (1) is 1 to 1.5 atm; Preferably, the temperature of the nitriding treatment in step (1) is 900-1100° C. Preferably, the nitriding treatment time in step (1) is 0.5 to 1.5 hours; Preferably, the nitriding treatment in step (1) is followed by cooling treatment and then oxidation treatment; Preferably, the oxygen flow rate of the oxidation treatment in step (1) is 100 to 300 mL / min; Preferably, the pressure of the oxidation treatment in step (1) is 1 to 1.5 atm; Preferably, the temperature of the oxidation treatment in step (1) is 400-500° C. Preferably, the oxidation treatment time in step (1) is 20 to 40 minutes.
7. The preparation method according to claim 5 or 6, characterized in that: The rare earth oxide in step (2) comprises lanthanum oxide; Preferably, the background vacuum degree of the first magnetron sputtering treatment in step (2) is 3×10 -5 Pa~6×10 -5 Pa; Preferably, the atmosphere of the first magnetron sputtering treatment in step (2) comprises argon and oxygen; Preferably, the flow ratio of argon to oxygen in step (2) is (1-5):1; Preferably, the gas pressure of the first magnetron sputtering treatment in step (2) is 0.5-0.8 Pa; Preferably, the power of the first magnetron sputtering treatment in step (2) is 100-140 W; Preferably, the time of the first magnetron sputtering treatment in step (2) is 0.5 to 2.5 hours.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The ferrite material in step (3) includes manganese-zinc ferrite; Preferably, the background vacuum degree of the second magnetron sputtering treatment in step (3) is 1×10 -3 Pa~5×10 -3 Pa; Preferably, the atmosphere of the second magnetron sputtering treatment in step (3) comprises argon; Preferably, in step (3), the gas pressure of the second magnetron sputtering treatment is 0.8 to 1.2 atm; Preferably, the sputtering power of the second magnetron sputtering treatment in step (3) is 150-250W; Preferably, in step (3), the vibration power of the second magnetron sputtering treatment is 20 to 40 W; Preferably, the time of the second magnetron sputtering treatment in step (3) is 2 to 4 hours.
9. A composite magnetic powder core, characterized in that: The composite magnetic powder core comprises the composite soft magnetic material according to any one of claims 1 to 4.
10. A method for preparing a composite magnetic powder core as claimed in claim 9, characterized in that: The preparation method comprises the following steps: The composite soft magnetic material is mixed with a binder, and then pressed and annealed to obtain the composite magnetic powder core; Preferably, the binder comprises any one of epoxy resin, phenolic resin or polyurethane resin or a combination of at least two thereof; Preferably, the mass ratio of the binder to the composite soft magnetic material is (0.5-2.5):100; Preferably, the pressing pressure is 20-25 T / cm 2 ; Preferably, the pressing time is 1 to 5 seconds; Preferably, the annealing temperature is 650-750°C; Preferably, the annealing treatment time is 0.5 to 1 hour.
Citation Information
Cited By
Preparation method and application of metal soft magnetic material
CN119833304A
Soft magnetic composite material, preparation method of soft magnetic composite material, preparation method of inductor and inductor
CN120690535A