High-strength magnetic shoe and preparation method thereof

By controlling the lifting angle of the green mold during the magnetic tile forming stage and using the inner arc grinding treatment of the inner arc fitting tool, the defects caused by large grinding amount are solved, and the compressive strength and pass rate of the magnetic tile are improved, so as to achieve Consistency between thickness and weight.

CN118919216APending Publication Date: 2024-11-08HUNAN AEROSPACE MAGNET & MAGNETO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411084989.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing magnetic tile processing technology, large grinding volume leads to magnetic tile prone to defects, low strength and high unqualification rate, and cumulative errors in the grinding process lead to inconsistency in thickness and weight, which cannot meet the requirements of high compressive strength.

Method used

By controlling the lifting angle of the foot on both sides of the green mold during the forming stage, the amount of grinding in the later stage is reduced, and the inner arc treatment is performed using tooling fitted with the inner arc of the blank to eliminate the accumulated errors caused by the arch height and external arc positioning. Ensure consistency of thickness and weight, thereby increasing the overall strength of the magnetic shingles.

Benefits of technology

It effectively reduces the adverse effects brought by grinding, improves the compressive strength and qualification rate of the magnetic shingles, ensures the consistency of thickness and weight of the magnetic shingles, and the maximum compressive strength can reach 3354N.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919216A_ABST
    Figure CN118919216A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength magnetic shoe and a preparation method thereof, and the method comprises the following steps: putting a green body material into a green body mold for molding, and lifting the two sides of the green body mold upwards to obtain a green body of which the two sides of the inner arc are lifted by 15-30 degrees; sintering the green body to obtain a blank; the blank is placed on a tool to be subjected to outer arc grinding treatment after being subjected to arch height forming treatment, a protrusion attached to the inner arc of the blank is arranged on the tool, finally, inner arc grinding treatment is conducted on the blank, and the high-strength magnetic shoe is obtained. The high-strength magnetic shoe is prepared by the preparation method. According to the method, the problems caused by grinding are reduced from the aspect of reducing the grinding amount, then accumulated errors are further reduced from the aspect of blank treatment, the thickness and weight consistency during magnetic shoe machining is effectively guaranteed, and therefore the qualification rate and the strength of the magnetic shoe are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic tile processing, and in particular to a high-strength magnetic tile and a preparation method thereof. Background Art

[0002] The processing of magnetic tiles generally involves sintering the wet-formed green body to form a blank with a certain strength and size, and then grinding the sintered blank into a standard size using a grinding wheel. The strength of the magnetic tile is related to the green body design and grinding process. The greater the amount of grinding on the blank, the higher the probability of defects such as falling blocks, cracks, and holes in the magnetic tile. When the magnetic tile is subjected to external force, stress concentration will occur near the defect, and the strength of the magnetic tile will be lower.

[0003] Existing embryo designs are as follows Figure 2 As shown in the figure, the green embryo is sintered to obtain the blank, and then the finished product is ground. For products with a large arch angle, the grinding amount is large; and the existing grinding process is used to position the thickness through the arch surface and the outer arc of the magnetic tile, such as Figure 4 As shown, this positioning method will have cumulative errors, and the thickness consistency of the magnetic tile is poor during grinding, resulting in poor consistency in the overall strength of the magnetic tile, which cannot meet the requirements for high compressive strength of the magnetic tile. In summary, the magnetic tile prepared by the prior art has a high failure rate and low strength. Summary of the invention

[0004] The purpose of the invention is to provide a high-strength magnetic tile and a preparation method thereof, which solves the problem that the magnetic tiles prepared by the prior art have a high failure rate and low strength.

[0005] The present invention is implemented in this way: a method for preparing a high-strength magnetic tile comprises the following steps:

[0006] Step 1: placing the green blank into a green blank mold for molding, and lifting the two sides of the green blank mold upward to obtain a green blank with the inner arc sides raised by 15°-30°;

[0007] Step 2, sintering the green body to obtain a blank;

[0008] Step three, after the blank is arched and raised, it is placed on a tooling to grind the outer arc. The tooling is provided with a protrusion that fits the inner arc of the blank. Finally, the blank is ground into the inner arc to obtain a high-strength magnetic tile.

[0009] In the existing method for preparing magnetic tiles, the preparation of magnetic tiles is to first make a green body, sinter it to obtain a blank, and grind it to obtain a magnetic tile that meets the requirements; in the final grinding stage, the greater the grinding amount, the more likely the magnetic tile will have defects, thereby causing problems with unqualified products or low strength; the present invention, firstly, controls the lifting of the feet on both sides of the green body in the forming stage to reduce the amount of grinding at this point in the later stage, and when combined with the later inner arc grinding treatment, the present invention adopts a tooling that fits the inner arc of the blank, and then performs inner arc grinding to process the blank thickness. Compared with the prior art, the cumulative errors caused by the arch height and the outer arc positioning are eliminated, and the thickness and weight consistency of the magnetic tile during processing can be effectively guaranteed, and the overall strength of the magnetic tile will be better; the present invention, firstly, reduces the problems caused by grinding by reducing the grinding amount, and then further reduces the cumulative errors from the blank processing, effectively ensuring the thickness and weight consistency of the magnetic tile during processing, thereby ensuring the qualification rate and strength of the magnetic tile.

[0010] A further technical solution of the present invention is: the molding pressure in step 1 is 340kg / cm 2 -480kg / cm 2 .

[0011] The larger the lifting angle of the magnetic tile, the less grinding amount, but it will increase the difficulty of forming and sintering, and the product failure rate will increase accordingly; the present invention has a molding pressure of 340kg / cm 2 -480kg / cm 2 Molding under this condition can effectively reduce the failure rate in the molding process.

[0012] A further technical solution of the present invention is: the sintering temperature range in the step 2 is 1100°C-1200°C.

[0013] The larger the lifting angle of the magnetic tile, although the grinding amount is less, the difficulty of forming and sintering will increase, and the product failure rate will increase accordingly; the present invention performs sintering at a sintering temperature range of 1100°C-1200°C, which can effectively reduce the failure rate during the sintering process.

[0014] A further technical solution of the present invention is: the arching processing step is to place the blank on the arching tooling, the outer arc of the blank fits with the groove of the arching tooling, and a rotatable grinding wheel is provided above the blank.

[0015] First, the arch heightening process is carried out, and the outer arc is matched with the groove of the arch heightening tooling, and the grinding wheel is used to grind the blank, which has high stability and strong operability.

[0016] A further technical solution of the present invention is: the outer arc grinding process is that the inner arc of the blank is fitted with the protrusion of the tooling, and a rotatable grinding piece that fits with the outer arc of the blank is provided on the outer arc of the blank.

[0017] When processing the inner arc of the blank, the inner arc of the blank is fitted with the protrusion of the tooling, and then the outer arc is polished. Compared with the prior art of placing the blank on a flat tooling for outer arc polishing, the present invention can eliminate the cumulative errors caused by the arch height and outer arc positioning, thereby ensuring the strength of the magnetic tile.

[0018] A further technical solution of the present invention is: the inner arc grinding process is to fit the outer arc of the green blank with the groove of the inner arc grinding tooling, and a rotatable inner arc grinding part that fits with the inner arc of the green blank is provided on the inner arc of the green blank.

[0019] When grinding the inner arc, the outer arc of the green blank fits into the groove on the inner arc grinding tooling, and then the inner arc grinding is performed. The grinding has high stability and high thickness consistency.

[0020] The present invention also provides a high-strength magnetic tile, which is prepared by the preparation method.

[0021] The magnetic tiles obtained by the preparation method of the present invention can firstly reduce the grinding amount, which can effectively reduce the adverse effects caused by grinding; secondly, the positioning design during grinding, the cumulative errors caused by the arch height and outer arc positioning can effectively ensure the consistency of the thickness and weight of the magnetic tiles during processing, and the overall strength of the magnetic tiles will be higher.

[0022] A further technical solution of the present invention is that the compressive strength of the high-strength magnetic tile can reach up to 3354N.

[0023] Beneficial effects of the present invention: in the existing method for preparing magnetic tiles, the preparation of magnetic tiles adopts the method of first making green billets, sintering to obtain blanks, and grinding to obtain magnetic tiles that meet the requirements; in the final grinding stage, the greater the grinding amount, the more likely the magnetic tiles will have defects, thereby causing problems such as unqualified products or low strength; the present invention, firstly, controls the lifting of the feet on both sides of the green billet in the forming stage to reduce the amount of grinding at this point in the later stage, and when combined with the later inner arc grinding treatment, the present invention adopts a tooling that fits the inner arc of the blank, and then performs inner arc grinding to process the blank thickness. Compared with the prior art, the cumulative errors caused by the arch height and the outer arc positioning are eliminated, and the thickness and weight consistency of the magnetic tiles during processing can be effectively guaranteed, and the overall strength of the magnetic tiles will be better; the present invention, firstly, reduces the problems caused by grinding by reducing the grinding amount, and then further reduces the cumulative errors from the blank processing, effectively ensuring the thickness and weight consistency of the magnetic tiles during processing, thereby ensuring the qualification rate and strength of the magnetic tiles. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a flow chart of the preparation method provided by the present invention;

[0025] Figure 2 It is a diagram of the state change of the magnetic tile corresponding to the preparation method of the prior art;

[0026] Figure 3 It is a diagram of the state change of the magnetic tile corresponding to the preparation method of the present invention;

[0027] Figure 4 It is a schematic diagram of the prior art grinding process;

[0028] Figure 5 It is a schematic diagram of the grinding process of the preparation method of the present invention.

[0029] Figure numerals: 1. magnetic tile, 11. grinding wheel, 12. arch heightening tooling, 21. grinding part, 22. tooling, 31. inner arc grinding part, 32. inner arc grinding tooling. DETAILED DESCRIPTION

[0030] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0031] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any modification of the structure, change of the proportion relationship or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. The change or adjustment of their relative relationship should also be regarded as the scope of the implementation of the present invention without substantially changing the technical content.

[0032] The present invention provides a method for preparing a high-strength magnetic tile, comprising the following steps:

[0033] Step 1: placing the green blank into a green blank mold for molding, and lifting the two sides of the green blank mold upward to obtain a green blank with the inner arc sides raised by 15°-30°;

[0034] Step 2, sintering the green body to obtain a blank;

[0035] Step three, after the blank is arched and raised, it is placed on a tooling to grind the outer arc, the tooling is provided with a protrusion that fits the inner arc of the blank, and finally the blank is ground with the inner arc to obtain a high-strength magnetic tile 1.

[0036] The molding pressure in step 1 is 340 kg / cm2 -480kg / cm 2 .

[0037] The sintering temperature range in step 2 is 1100°C-1200°C.

[0038] The arching step is to place the blank on the arching tool 12, so that the outer arc of the blank fits the groove of the arching tool 12, and a rotatable grinding wheel 11 is arranged above the blank. The grinding wheel 11 rotates on a horizontal plane.

[0039] The outer arc grinding process is that the inner arc of the blank is fitted with the protrusion of the tooling 22, and a rotatable grinding piece 21 is provided on the outer arc of the blank to fit with the outer arc of the blank.

[0040] The inner arc grinding process is to fit the outer arc of the green blank into the groove of the inner arc grinding tool 32, and a rotatable inner arc grinding part 31 that fits the inner arc of the green blank is provided on the inner arc of the green blank.

[0041] The specific implementation methods of the present invention are as follows:

[0042] Embodiment 1:

[0043] A method for preparing a high-strength magnetic tile comprises the following steps:

[0044] Step 1: Place the green blank into a green blank mold for molding, and lift the two sides of the green blank mold upward to obtain a green blank with the inner arc raised by 15° on both sides;

[0045] Step 2, sintering the green body to obtain a blank;

[0046] Step three, after the blank is arched and raised, it is placed on a tooling to grind the outer arc. The tooling is provided with a protrusion that fits the inner arc of the blank. Finally, the blank is ground into the inner arc to obtain a high-strength magnetic tile.

[0047] In this embodiment, the molding pressure in step 1 is 340 kg / cm 2 .

[0048] In this embodiment, the sintering temperature range in step 2 is 1100°C.

[0049] In this embodiment, the arching processing step is to place the blank on the arching tooling, so that the outer arc of the blank fits with the groove of the arching tooling, and a rotatable grinding wheel is provided above the blank.

[0050] In this embodiment, the outer arc grinding process is that the inner arc of the blank is fitted with the protrusion of the tooling, and a rotatable grinding piece that fits with the outer arc of the blank is provided on the outer arc of the blank.

[0051] In this embodiment, the inner arc grinding process is to fit the outer arc of the green blank with the groove of the inner arc grinding tooling, and a rotatable inner arc grinding part that fits with the inner arc of the green blank is provided on the inner arc of the green blank.

[0052] The magnetic tiles obtained in this embodiment were subjected to a compressive strength test. The finished products were tested for compressive strength every other day. A total of 10 batches of compressive strength tests were conducted, with five samples taken from each batch. The results are shown in Table 1.

[0053] Table 1 Compressive strength of finished product of Example 1 (N)

[0054]

[0055] It can be seen from Table 1 that the highest compressive strength of the magnetic tile obtained in Example 1 can reach 3354N; the maximum average compressive strength is 2949.8N.

[0056] Embodiment 2:

[0057] A method for preparing a high-strength magnetic tile comprises the following steps:

[0058] Step 1: Place the green blank into a green blank mold for molding, and lift the two sides of the green blank mold upward to obtain a green blank with the inner arc raised by 25 degrees on both sides;

[0059] Step 2, sintering the green body to obtain a blank;

[0060] Step three, after the blank is arched and raised, it is placed on a tooling to grind the outer arc. The tooling is provided with a protrusion that fits the inner arc of the blank. Finally, the blank is ground into the inner arc to obtain a high-strength magnetic tile.

[0061] In this embodiment, the molding pressure in step 1 is 420 kg / cm 2 .

[0062] In this embodiment, the sintering temperature range in step 2 is 1150°C.

[0063] In this embodiment, the arching processing step is to place the blank on the arching tooling, so that the outer arc of the blank fits with the groove of the arching tooling, and a rotatable grinding wheel is provided above the blank.

[0064] In this embodiment, the outer arc grinding process is that the inner arc of the blank is fitted with the protrusion of the tooling, and a rotatable grinding piece that fits with the outer arc of the blank is provided on the outer arc of the blank.

[0065] In this embodiment, the inner arc grinding process is to fit the outer arc of the green blank with the groove of the inner arc grinding tooling, and a rotatable inner arc grinding part that fits with the inner arc of the green blank is provided on the inner arc of the green blank.

[0066] Through this embodiment, 5 magnetic tiles are prepared at the same time, and the product thickness and weight are highly consistent. The finished product obtained in this embodiment is tested for compressive strength, and the average compressive strength is 2630N.

[0067] Embodiment three:

[0068] A method for preparing a high-strength magnetic tile comprises the following steps:

[0069] Step 1: Place the green blank into a green blank mold for molding, and lift the two sides of the green blank mold upward to obtain a green blank with the inner arc raised by 30° on both sides;

[0070] Step 2, sintering the green body to obtain a blank;

[0071] Step three, after the blank is arched and raised, it is placed on a tooling to grind the outer arc. The tooling is provided with a protrusion that fits the inner arc of the blank. Finally, the blank is ground into the inner arc to obtain a high-strength magnetic tile.

[0072] In this embodiment, the molding pressure in step 1 is 480 kg / cm 2 .

[0073] In this embodiment, the sintering temperature range in step 2 is 1200°C.

[0074] In this embodiment, the arching processing step is to place the blank on the arching tooling, so that the outer arc of the blank fits with the groove of the arching tooling, and a rotatable grinding wheel is provided above the blank.

[0075] In this embodiment, the outer arc grinding process is that the inner arc of the blank is fitted with the protrusion of the tooling, and a rotatable grinding piece that fits with the outer arc of the blank is provided on the outer arc of the blank.

[0076] In this embodiment, the inner arc grinding process is to fit the outer arc of the green blank with the groove of the inner arc grinding tooling, and a rotatable inner arc grinding part that fits with the inner arc of the green blank is provided on the inner arc of the green blank.

[0077] Through this embodiment, 5 magnetic tiles are prepared at the same time, and the product thickness and weight are highly consistent. The finished product obtained in this embodiment is tested for compressive strength, and the average compressive strength is 2750N.

[0078] Comparative Example 1:

[0079] The difference from the first embodiment is that when forming in the green mold, the green mold for placing the green material is flat and has no lifting foot design; Figure 2 shown.

[0080] Five magnetic tiles were prepared at the same time by this comparative example, and there was a situation of falling off during grinding; the finished product obtained in this comparative example was tested for compressive strength, and the average compressive strength was 2180 N. Example 1 Compared with this comparative example, Example 1 can effectively reduce the grinding amount of the blank arch height position (reducing the grinding amount by about 4%), and reduce the probability of defects such as falling off during blank grinding.

[0081] Comparative Example 2:

[0082] The difference from the first embodiment is that in step 3, the blank is placed on a tooling for outer arc grinding after arching, the surface of the tooling is flat, and finally the blank is ground for inner arc grinding to obtain a high-strength magnetic tile. Figure 4 shown.

[0083] Through this comparative example, 5 magnetic tiles were prepared at the same time, and there were visible differences in the thickness of the 5 products, and the consistency of thickness and weight was low; the finished products obtained in this comparative example were tested for compressive strength, and the average compressive strength was 2140N.

[0084] Comparative Example 3:

[0085] The difference from the first embodiment is that when forming in the green mold, the green mold for placing the green material is flat and has no lifting foot design; Figure 2 shown.

[0086] In step three, the blank is placed on a tooling for external arc grinding after arching, and the surface of the tooling is flat. Finally, the blank is ground internally to obtain a high-strength magnetic tile. Figure 4 shown.

[0087] The magnetic tiles obtained in this comparative example were subjected to a compressive strength test. The finished products were tested for compressive strength every day. A total of 10 batches of compressive strength tests were conducted, with five samples taken from each batch. The results are shown in Table 2.

[0088] Table 2 Comparative Example 1 Compressive Strength of Finished Product (N)

[0089]

[0090] It can be seen from Table 2 that the maximum average compressive strength is 2246N.

[0091] Compared with the comparative example, the embodiment 1 can effectively reduce the grinding amount of the blank arch height position (reducing the grinding amount by about 4%), and reduce the probability of defects such as block drop during blank grinding. In addition, the thickness and weight of the finished product of the embodiment 1 are consistent, and the strength is increased by about 700N compared with the comparative example.

[0092] Comparative Example 4:

[0093] The difference from Example 1 is that the molding pressure in step 1 is 280 kg / cm 2 The sintering temperature of step 2 is 800°C.

[0094] Through this comparative example, 5 magnetic tiles were prepared at the same time, one of which could not be formed, and the remaining four were subjected to a compressive strength test, with an average compressive strength of 1380N.

[0095] Comparative Example 5:

[0096] The difference from Example 1 is that the molding pressure in step 1 is 600 kg / cm 2 The sintering temperature of step 2 is 2200°C.

[0097] Through this comparative example, 5 magnetic tiles were prepared at the same time, and each magnetic tile had different degrees of chipping. The finished products obtained in this comparative example were tested for compressive strength, and the average compressive strength was 920N.

[0098] In summary, the present invention first reduces the problems caused by grinding by reducing the amount of grinding, and then further reduces the cumulative error from the blank processing, effectively ensuring the consistency of thickness and weight during the processing of the magnetic tile, thereby ensuring the qualification rate and strength of the magnetic tile. Since raising the forming mold will cause the difficulty of forming and sintering, the product qualification rate will increase. The forming and sintering adopted by the present invention can ensure the product qualification rate.

[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-strength magnetic tile, characterized in that: The following steps are involved: Step 1: placing the green blank into a green blank mold for molding, and lifting the two sides of the green blank mold upward to obtain a green blank with the inner arc sides raised by 15°-30°; Step 2, sintering the green body to obtain a blank; Step three, after the blank is arched and raised, it is placed on a tooling to grind the outer arc. The tooling is provided with a protrusion that fits the inner arc of the blank. Finally, the blank is ground into the inner arc to obtain a high-strength magnetic tile.

2. The method for preparing a high-strength magnetic tile according to claim 1, characterized in that: The molding pressure in step 1 is 340 kg / cm 2 -480kg / cm 2 .

3. The method for preparing a high-strength magnetic tile according to claim 1, characterized in that: The sintering temperature range in step 2 is 1100°C-1200°C.

4. The method for preparing a high-strength magnetic tile according to claim 1, characterized in that: The arching and raising processing step is to place the blank on the arching and raising tooling, so that the outer arc of the blank fits with the groove of the arching and raising tooling, and a rotatable grinding wheel is arranged above the blank.

5. The method for preparing a high-strength magnetic tile according to claim 1, characterized in that: The outer arc grinding process is that the inner arc of the blank is fitted with the protrusion of the tooling, and a rotatable grinding piece that fits with the outer arc of the blank is provided on the outer arc of the blank.

6. The method for preparing a high-strength magnetic tile according to claim 1, characterized in that: The inner arc grinding process is to fit the outer arc of the green blank with the groove of the inner arc grinding tooling, and a rotatable inner arc grinding part that fits with the inner arc of the green blank is provided on the inner arc of the green blank.

7. A high-strength magnetic tile, characterized in that: The high-strength magnetic tile is prepared by the preparation method described in any one of claims 1-6.

8. The high-strength magnetic tile according to claim 7, characterized in that: The compressive strength of the high-strength magnetic tile can reach up to 3354N.