Preparation method of square nanocrystalline magnetic core common mode inductor

Through the preparation method of square nanocrystalline magnetic core common mode inductance, the circular ring core is transformed into a rectangular structure, which solves the problem of uneven flux paths and improves the processing convenience and use performance of the magnetic core.

CN118919273AActive Publication Date: 2024-11-08FOSHAN HUAXIN MICROCRYSTALLINE METAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410991523.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

During the processing of nanocrystalline magnetic core, the flux paths of the circular magnetic core are uneven, resulting in difficulty in subsequent winding, reduced efficiency and increased losses.

Method used

The preparation method of square nanocrystalline magnetic core common mode inductor is adopted, including incoming material inspection, stacking and shaping, end surface flattening, heat treatment, paint immersion treatment, curing and shaping and surface treatment steps, and transform the circular ring core into a rectangular structure to ensure that The flux path is uniform.

Benefits of technology

It realizes convenient processing of the magnetic core and uniform flux path, reduces the difficulty of winding, and improves the performance and stability of the magnetic core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919273A_ABST
    Figure CN118919273A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nanocrystalline magnetic core preparation, in particular to a preparation method of a square nanocrystalline magnetic core common mode inductor, which comprises the following construction steps: incoming material inspection, overlying and shaping, end face flattening, heat treatment, paint dipping treatment, curing and shaping, and surface treatment. The magnetic core can be converted into a rectangular structure from an annular structure easy to produce, the converted structure is stable in mechanical performance, not prone to springback and good in finished product quality, the magnetic flux path of the magnetic core of the rectangular structure also becomes uniform, it can be guaranteed that the amorphous nanocrystalline magnetic core is convenient to machine, meanwhile, the magnetic flux path of the magnetic core is uniform, the winding difficulty is reduced, and the production efficiency is improved. The use performance of the magnetic core is enhanced, and production requirements are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nanocrystalline magnetic core preparation, and in particular to a method for preparing a square nanocrystalline magnetic core common mode inductor. Background Art

[0002] Nanocrystalline magnetic core is a soft magnetic structure with nanoscale crystal structure. The alloy is directly formed into amorphous thin strip from molten state through rapid cooling technology, and then the amorphous state is transformed into nanocrystalline state through heat treatment. Nanocrystalline magnetic core is mainly used in power electronics fields such as common mode inductors, high frequency transformers, current transformers, drive transformers, etc.

[0003] At present, in the processing of nanocrystalline magnetic cores, an amorphous nanocrystalline magnetic core is taken and heat treated at a temperature of about 400°C. Then nitrogen is introduced into the furnace for 8-10 hours to transform the amorphous state into the nanocrystalline state to obtain a nanocrystalline magnetic core.

[0004] However, in actual applications, in order to facilitate shearing processing, amorphous nanocrystalline magnetic cores are often designed into a ring shape. However, the magnetic flux path of the ring-shaped magnetic core is poor, and it is difficult to wind the wire evenly during the subsequent coil winding, which leads to reduced efficiency and increased losses of the magnetic core. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art of the above-mentioned background technology, the present application provides a method for preparing a square nanocrystalline magnetic core common-mode inductor, which can ensure the convenient processing of amorphous nanocrystalline magnetic cores, while making the magnetic flux path of the magnetic core uniform, reducing the difficulty of winding, and enhancing the performance of the magnetic core.

[0006] The present application provides a method for preparing a square nanocrystalline magnetic core common mode inductor, which adopts the following technical solution: A method for preparing a square nanocrystalline magnetic core common mode inductor comprises the following steps: S1: Incoming material inspection: The surface of each core material is free of burrs and kept dry, and the single-side thickness of the core material is controlled within the specified range; S2: stacking and shaping: inserting the core into the first pressing sheet, stacking a plurality of the magnetic core materials on the first pressing sheet in sequence, placing the core in the middle of the magnetic core materials, and then taking the second pressing sheet and setting it at an end away from the first pressing sheet, the second pressing sheet is plugged into the core to obtain a stacked combined structure; S3: end surface flattening: placing a plurality of the stacked combined structures in a fixture in sequence, spacing two adjacent stacked combined structures by a clamp, and flattening the end surfaces of the plurality of stacked combined structures simultaneously by a pressing assembly; S4: heat treatment: placing the laminated composite structure in a heat treatment furnace for heat treatment; S5: varnishing treatment: placing the laminated composite structure after heat treatment in a vacuum pressure varnishing device for varnishing treatment; S6: curing and shaping: baking and curing the laminated composite structure after varnishing, then disassembling the laminated composite structure from the fixture, and then decomposing the cured and shaped magnetic core raw material, the first pressing sheet, the second pressing sheet, and the core, and shaping the cured and shaped magnetic core raw material into a nanocrystalline magnetic core; S7: Surface treatment: removing redundant insulating paint on the surface of the nanocrystalline magnetic core, and performing surface loss reduction treatment and surface protection treatment on the nanocrystalline magnetic core to obtain the finished magnetic core.

[0007] By adopting the above technical scheme, the quality of the raw materials is ensured by strictly screening the raw materials of the magnetic core, which is burr-free, dry and within the specified thickness range, which helps to ensure the performance and stability of the final product. The stacking and shaping method is adopted so that multiple magnetic core materials can be stacked tightly and neatly together. At the same time, the flatness and consistency of the magnetic core materials are ensured by end face flattening treatment. Affected by the material of the magnetic core raw materials, the magnetic core raw materials are deformed after being subjected to pressure, so that the annular magnetic core is transformed into a rectangular magnetic core. Through heat treatment, the internal organizational structure of the magnetic core can be improved, and its mechanical properties and magnetic properties can be improved. The varnishing treatment can enhance the insulation performance and corrosion resistance of the magnetic core. The baking and curing makes the varnishing layer more firmly attached to the surface of the magnetic core to improve the durability and reliability of the magnetic core, thereby realizing the transformation from amorphous nanocrystalline magnetic core to nanocrystalline magnetic core, while maintaining the shaping without restoring the deformation. Finally, by removing the redundant insulating paint, surface loss reduction treatment and surface protection treatment are performed, the surface quality of the magnetic core is further optimized, which helps to reduce the loss caused by friction and corrosion during use.

[0008] Compared with the prior art, through the processing steps of incoming material inspection, lamination and shaping, end face flattening, heat treatment, paint dipping, curing and shaping, and surface treatment, it is possible to realize batch processing of magnetic core raw materials, so that it can be transformed from an easy-to-produce ring structure into a rectangular structure, and the mechanical properties of the transformed structure are stable, it is not prone to springback, the finished product quality is good, and the magnetic flux path of the rectangular structure magnetic core becomes uniform. After the above steps are processed, it can ensure that the processing of amorphous nanocrystalline magnetic cores is convenient, and at the same time, the magnetic flux path of the magnetic core is uniform, the difficulty of winding is reduced, the performance of the magnetic core is enhanced, and it meets production needs.

[0009] Preferably, in the processing step S2, the shapes and structures of the first pressed sheet and the second pressed sheet are consistent, and are twice the weight of the magnetic core raw material.

[0010] By adopting the above technical scheme, in the stacking and shaping step of preparing the rectangular nanocrystalline magnetic core common-mode inductor, the shape structure of the first pressing plate and the second pressing plate are consistent, which can ensure that uniform pressure is applied to the magnetic core raw material during the stacking process, thereby obtaining a more regular and compact stacking combination structure, which helps to improve the accuracy and consistency of the magnetic core, and provides a guarantee for subsequent processing and final product performance.

[0011] Secondly, the weight of the first pressing sheet and the second pressing sheet is designed to be twice that of the core material. This ratio helps to generate sufficient pressure during the stacking process, so that the core materials are more tightly combined together, which can enhance the structural strength of the core, reduce internal gaps, and improve the electrical performance of the core.

[0012] Preferably, the core comprises at least two core bodies, the core bodies are detachably connected to each other, and the core has a rectangular structure as a whole.

[0013] By adopting the above technical solution, during the preparation process, the rectangular core can provide stable support and positioning for the core material, thereby ensuring that the shape and size of the core meet the requirements, which helps to ensure the accuracy and consistency of the core.

[0014] Secondly, the detachable core design provides good flexibility and convenience, allowing the core to be quickly assembled and disassembled according to specific needs, which helps to simplify the preparation process and greatly improve production efficiency. It also facilitates the maintenance and replacement of the core to reduce the cost of use.

[0015] Preferably, the core comprises a first core body, a second core body and a third core body, the first core body and the second core body are right-angled trapezoidal structures with consistent shapes and sizes, the third core body is an isosceles trapezoidal structure, the first core body, the second core body and the third core body are arranged at the same height, in the processing step S2, one waist surface of the third core body abuts against the inclined surface of the first core body, and the other waist surface of the third core body abuts against the inclined surface of the second core body, and the three are assembled to form a rectangular structure, the outer edges of the first core body and the second core body are rounded and at the same time abut against the inner wall of the magnetic core raw material.

[0016] By adopting the above technical solution, the first core body and the second core body are designed as right-angled trapezoidal structures with consistent shapes and sizes, and the third core body is an isosceles trapezoidal structure. This design enables the three core bodies to be tightly assembled together to form a stable rectangular structure, thereby providing uniform support force for the magnetic core material and ensuring the flatness and consistency of the magnetic core.

[0017] In addition, the outer edges of the first core body and the second core body are rounded, which can reduce the stress concentration generated during the processing, improve the fatigue strength and service life of the magnetic core, help improve the appearance quality of the magnetic core, and help improve the electrical performance of the magnetic core.

[0018] Preferably, the processing step of S4 includes the following steps: S4.1: first evacuate the cavity of the heat treatment furnace, and then introduce inert gas into the cavity; S4.2: When the temperature reaches the starting temperature, place the entire fixture in the cavity; S4.3: setting at least one preset temperature node, gradually increasing the temperature in sequence, and maintaining the temperature for a period of time until the last preset temperature node is reached; at the same time, adding a magnetic field to the cavity; S4.4: Cool down to a cooling temperature node.

[0019] By adopting the above technical solution, by first evacuating the heat treatment furnace chamber and then introducing inert gas, the chemical reaction of the magnetic core material with oxygen or other active gases in the air during the heat treatment process can be effectively reduced to ensure the purity and performance stability of the magnetic core; by setting multiple preset temperature nodes and gradually increasing the temperature in sequence, while increasing the magnetic field at a specific temperature, this treatment method can finely control the microstructure and magnetic properties of the magnetic core, and realize the transformation from an amorphous nanocrystalline magnetic core to a nanocrystalline magnetic core. In addition, the gradual increase in temperature during the heat treatment process helps to reduce the thermal stress of the magnetic core to prevent the magnetic core from cracking or deforming during the heat treatment process. Finally, the temperature is reduced to a cooling temperature node to ensure that the magnetic core can be slowly cooled after the heat treatment, avoiding internal stress caused by rapid cooling, and further ensuring the quality and performance of the magnetic core.

[0020] Preferably, the inert gas includes nitrogen and argon. In the processing step S4.1, when the temperature in the heat treatment furnace is below 500°C, nitrogen is introduced; when the temperature in the heat treatment furnace is above 500°C, argon is introduced.

[0021] By adopting the above-mentioned technical scheme, the introduction of nitrogen or argon can be flexibly selected according to the temperature in the heat treatment furnace, so that the magnetic core material can be better protected from oxidation or other chemical reactions. Moreover, the present application utilizes the characteristics that nitrogen and argon have different protective effects at different temperatures, making the protection effect more precise and efficient, and can effectively reduce the contamination and oxide layer formation on the surface of the magnetic core, thereby improving the quality and electrical performance of the magnetic core.

[0022] Preferably, in the processing step S4.3, the temperature in the heat treatment furnace is maintained at 480° C. for 12 hours.

[0023] By adopting the above technical solution and maintaining it at 480°C for 12 hours, the atoms inside the core material can have enough time and energy to rearrange and adjust the structure, optimize its microstructure, improve the magnetic and mechanical properties, help eliminate stress and defects inside the material, and improve the uniformity and consistency of the core, thereby ensuring that the core material reaches a stable crystal structure state, thereby improving its stability during use.

[0024] Preferably, in the processing step S4.4, when the magnetic core raw material that has been solidified and shaped is taken out of the heat treatment furnace, the temperature of the nanocrystalline magnetic core is maintained above 300°C.

[0025] By adopting the above technical solution, the magnetic core is taken out at a certain high temperature, and the remaining heat can be used for subsequent surface treatment or other steps requiring heat assistance, thereby improving energy efficiency and processing efficiency. In addition, the thermal stress caused by rapid temperature changes can be reduced, thereby reducing the risk of cracking or deformation of the magnetic core, and ensuring the quality and performance of the magnetic core.

[0026] Preferably, in the processing step of S5, the laminated composite structure is first immersed in the hardening liquid for 1 minute and then drained for 30 minutes until the hardening liquid penetrates into the microstructure of the magnetic core raw material; in the processing step of S6, the laminated composite structure after the paint is placed in a drying furnace for baking, and the temperature in the drying furnace is maintained at 140°C for 10 hours.

[0027] By adopting the above technical solution, the hardening liquid can fill the tiny pores inside the material, improve the density and mechanical properties of the material, and by immersing the laminated composite structure in the hardening liquid and preventing the hardening liquid from penetrating into the microstructure of the core raw material, the hardness and wear resistance of the core can be enhanced; drying at 140°C for 10 hours can ensure that the hardening liquid is evenly solidified inside the core to form a stable structure.

[0028] Preferably, after the processing step S7, spraying treatment is performed on 20-30 μm of the surface of the nanocrystalline magnetic core.

[0029] By adopting the above technical solution, a uniform and dense protective layer can be formed on the surface of the nanocrystalline magnetic core through spraying treatment. The protective layer can effectively isolate oxygen, moisture and other corrosive substances in the external environment, thereby extending the service life of the magnetic core. In addition, the spraying thickness is controlled within the range of 20-30μm, which can ensure that the protective layer has sufficient thickness to provide good protection effect, and avoid performance degradation or cost increase caused by excessively thick coating.

[0030] In summary, the present application includes at least one of the following beneficial technical effects: 1. Compared with the prior art, after the processing steps of incoming material inspection, lamination and shaping, end face flattening, heat treatment, varnishing treatment, curing and shaping, and surface treatment, the raw materials of the magnetic core can be processed in batches, so that it can be transformed from an easily produced ring structure to a rectangular structure, and the mechanical properties of the transformed structure are stable, and it is not easy to rebound. The finished product has good quality, and the magnetic flux path of the magnetic core of the rectangular structure becomes uniform. After the above steps, the processing of the amorphous nanocrystalline magnetic core can be ensured to be convenient, and at the same time, the magnetic flux path of the magnetic core is uniform, the difficulty of winding is reduced, and the performance of the magnetic core is enhanced, which meets the production requirements; 2. The detachable core design provides good flexibility and convenience, allowing the core to be quickly assembled and disassembled according to specific needs, which helps to simplify the preparation process and greatly improve production efficiency. It also facilitates the maintenance and replacement of the core to reduce the cost of use; 3. According to the temperature in the heat treatment furnace, flexibly choosing to introduce nitrogen or argon can better protect the magnetic core material from oxidation or other chemical reactions. Moreover, the present application utilizes the characteristics that nitrogen and argon have different protective effects at different temperatures, making the protection effect more accurate and efficient, which can effectively reduce the contamination and oxide layer formation on the surface of the magnetic core, thereby improving the quality and electrical performance of the magnetic core. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the structure of the magnetic core material in the embodiment of the present application.

[0032] Figure 2 It is an exploded view of the stacked combination structure in the embodiment of the present application.

[0033] Figure 3 It is a structural schematic diagram of a core in an embodiment of the present application.

[0034] Figure 4 It is a structural schematic diagram of a material pressing component in an embodiment of the present application.

[0035] Figure 5 It is a structural schematic diagram of another material pressing component in the embodiment of the present application.

[0036] Explanation of the reference numerals in the accompanying drawings: 1. laminated structure; 11. core material; 12. first pressing sheet; 13. second pressing sheet; 14. core; 141. first core body; 142. second core body; 143. third core body; 144. lifting rod; 1441. lifting part; 1442. connecting part; 1443. plug-in part; 2. clamp; 3. pressing plate; 4. pressing assembly; 411. first pressure plate; 412. threaded rod; 413. locking nut; 421. second pressure plate; 422. adjusting rod; 423. buffer; 424. driven bevel gear; 425. mounting seat; 426. driving shaft; 427. driving bevel gear. DETAILED DESCRIPTION

[0037] The following is combined with Figure 1-5 This application is described in further detail.

[0038] The embodiment of the present application discloses a method for preparing a square nanocrystalline magnetic core common mode inductor.

[0039] Reference Figure 1 and Figure 2 , a method for preparing a square nanocrystalline magnetic core common mode inductor, comprising the following construction steps: S1: Incoming material inspection: The surface of each magnetic core material 11 is free of burrs and kept dry, and the single-side thickness of the magnetic core material 11 is controlled within a specified range.

[0040] In the present application, the thickness of the strip is checked and controlled within 16-18, the surface cannot have burrs, the raw material storage cannot be exposed to moisture, and oxidation and rust of the strip are avoided. The strip is then divided into strips, and the width after dividing is 8mm. Similarly, the surface of the strip is free of burrs and other abnormalities. The strip is then wound to obtain a circular amorphous nanocrystalline magnetic core, and the single-side thickness of the magnetic core is 5mm, which is also referred to as magnetic core raw material 11 in the present application. It itself has high toughness and elasticity. The circular structure does not need to consider the corner angle, and the winding speed is fast. In the processing step of S1, multiple strips are uniformly wound into circular amorphous nanocrystalline magnetic cores with consistent structures to effectively improve production efficiency.

[0041] S2: Stacking and shaping: Insert the core 14 into the first pressing sheet 12, and stack multiple magnetic core materials 11 on the first pressing sheet 12 in sequence, so that the core 14 is placed in the middle of the magnetic core material 11, and then take the second pressing sheet 13 and set it at the end away from the first pressing sheet 12, and the second pressing sheet 13 is plugged into the core 14 to obtain a stacked combined structure 1.

[0042] Specifically, the first pressing sheet 12 and the second pressing sheet 13 have the same shape and structure, and are twice the weight of the magnetic core material 11 . The core 14 includes at least two core bodies, which are detachably connected to each other, and the core 14 has a rectangular structure as a whole.

[0043] The present application provides a preferred core 14 structure, referring to Figure 2The core 14 includes a first core body 141, a second core body 142 and a third core body 143. The first core body 141 and the second core body 142 are right-angled trapezoidal structures with the same shape and size, and the third core body 143 is an isosceles trapezoidal structure. The first core body 141, the second core body 142 and the third core body 143 are arranged at the same height, so that one waist surface of the third core body 143 abuts against the inclined surface of the first core body 141, and the other waist surface of the third core body 143 abuts against the inclined surface of the second core body 142. After the three are assembled, a rectangular structure is formed, and the outer edges of the first core body 141 and the second core body 142 are rounded.

[0044] When in use, first insert the large end of the first core 141 and the large end of the second core 142 into the first pressing sheet 12, then hang a plurality of magnetic core materials 11 outside the first core 141 and the second core 142, then take the third core 143 and insert its small end between the large end of the first core 141 and the large end of the second core 142 until one waist surface of the third core 143 abuts against the inclined surface of the first core 141, and the other waist surface of the third core 143 abuts against the inclined surface of the first core 141. The waist surface is in contact with the inclined surface of the second core body 142, and the three are assembled to form a rectangular structure, and the elastic annular magnetic core material 11 is extruded into a rectangular magnetic core material 11. At this time, the inner wall of the magnetic core material 11 is completely fitted with the core 14, and finally the second pressing sheet 13 is plugged into the core 14. Under the joint action of the first pressing sheet 12 and the second pressing sheet 13, multiple magnetic core materials 11 can be squeezed together so that the end faces of two adjacent magnetic core materials 11 can fit together.

[0045] In the present application, the first core 141 and the second core 142 are designed to be right-angled trapezoidal structures of consistent shape and size, while the third core 143 is an isosceles trapezoidal structure. This design enables the three cores to be tightly assembled together to form a stable rectangular structure, thereby providing uniform support for the magnetic core material 11 and ensuring the flatness and consistency of the magnetic core.

[0046] In addition, the outer edges of the first core body 141 and the second core body 142 are rounded, which can reduce the stress concentration generated during the processing, improve the fatigue strength and service life of the magnetic core, help improve the appearance quality of the magnetic core, and help improve the electrical performance of the magnetic core.

[0047] This application provides another preferred core 14 structure, referring to Figure 3On the basis of the previous core 14, the inclined surfaces of the first core body 141 and the inclined surfaces of the second core body 142 are respectively provided with guide grooves, and correspondingly, guide blocks (not shown in the figure) are respectively fixed on the two waist surfaces of the third core body 143. When the first core body 141, the second core body 142 and the third core body 143 are assembled, the two guide blocks are respectively adapted and slidably connected with the guide grooves close to them, so that the gap between the first core body 141 and the third core body 143, and the gap between the second core body 142 and the third core body 143 tend to zero.

[0048] Furthermore, an installation groove and a slide groove are opened inside the third core body 143. The extension direction of the installation groove is consistent with the length direction of the third core body 143. There are two slide grooves and they are symmetrically arranged along the center line of the installation groove. The slide groove penetrates from the end of the installation groove toward the first core body 141 or the second core body 142. Correspondingly, an extension groove is opened at a position of the first core body 141 near the slide groove and a position of the second core body 142 near the slide groove, respectively, and the extension groove and the slide groove are on the same extension line.

[0049] A lifting rod 144 is arranged in the installation groove, and the lifting rod 144 includes a lifting part 1441, a connecting part 1442 and a plug-in part 1443, wherein the lifting part 1441 is assembled with the connecting part 1442 through a bearing, and there are two plug-in parts 1443, which are respectively fixed on both sides of the connecting part 1442. In the present application, the plug-in part 1443 includes two parts of nodes, and the nodes and the connecting part 1442 are hinged and fixed. At the same time, the nodes of the plug-in part 1443 away from the connecting part 1442 are slidably connected with the sliding grooves close to them. In addition, an external thread is provided on the outer wall of the end of the lifting part 1441 away from the connecting part 1442. In the present application, the end of the lifting part 1441 provided with the external thread faces the large end of the third core 143.

[0050] When in use, after the first core 141, the second core 142 and the third core 143 are assembled, the lifting part 1441 is rotated by a tightening tool to lower the lifting part 1441, and the plug-in part 1443 slides along the slide groove until it transitions to the extension groove, further improving the connection density of the three and greatly improving the stable connection of the three.

[0051] In the stacking and molding step of S2 of the present application, the rectangular core 14 can provide stable support and positioning for the magnetic core raw material 11, thereby ensuring that the shape and size of the magnetic core meet the requirements, and the detachable core design provides good flexibility and convenience, so that the core 14 can be quickly assembled and disassembled according to specific needs, which helps to simplify the preparation process, improve production efficiency, and facilitate maintenance and replacement of the core 14 to reduce the cost of use.

[0052] At the same time, the shape and structure of the first pressing plate 12 and the second pressing plate 13 are consistent, which can ensure that uniform pressure is applied to the magnetic core material 11 during the stacking process, so as to obtain a more regular and compact stacked combination structure 1, and the weight of the first pressing plate 12 and the second pressing plate 13 is designed to be twice that of the magnetic core material 11. This ratio helps to generate sufficient pressure during the stacking process, so that the magnetic core material 11 is more closely combined together, which helps to improve the accuracy and consistency of the magnetic core, and provides a guarantee for subsequent processing and final product performance.

[0053] In the present application, the core 14, the first pressing plate 12 and the second pressing plate 13 are all made of iron materials. The magnetic core raw material 11 itself has good magnetic properties. By utilizing its own properties, the structures have a certain attraction ability, thereby enhancing the overall structural stability of the laminated combination structure 1.

[0054] S3: end face flattening: multiple stacked composite structures 1 are placed in the fixture 2 in sequence. The fixture 2 is in the shape of a rectangular frame. The side walls of the fixture 2 are all steel plates with through holes, and the multiple through holes are evenly arranged. Two adjacent stacked composite structures 1 are spaced apart by a clamp. The end faces of the multiple stacked composite structures 1 are flattened at the same time by the pressing assembly 4.

[0055] The present application provides a preferred structure of a pressing component 4, referring to Figure 4 , including a first pressure plate 411, a threaded rod 412 and a locking nut 413, wherein the outer wall of the threaded rod 412 is provided with an external thread, the threaded rod 412 passes through one of the through holes, the first pressure plate 411 is fixed to the end of the threaded rod 412 and arranged in the fixture 2, so that the adjacent side walls of the first pressure plate 411 are parallel to each other and perpendicular to the extension direction of the threaded rod 412, and each threaded rod 412 is provided with two locking nuts 413, when the first pressure plate 411 is in contact with the side wall of the stacked composite structure 1, the two locking nuts 413 are rotated, so that the position of the threaded rod 412 and the first pressure plate 411 can be limited. In the present application, each side wall of the fixture 2 is provided with a set of pressing components 4, so that the multiple sets of stacked composite structures 1 placed in the four first pressure plates 411 can be squeezed by the clamp until the outer end surface of the core material 11 is flattened, thereby forming a rectangular core material 11 with a more stable structure.

[0056] This application provides another preferred structure of the pressing component 4, referring to Figure 5 , a second pressure plate 421 and an adjusting rod 422, wherein there are two second pressure plates 421 and two adjusting rods 422, one end of the outer wall of the adjusting rod 422 is provided with a positive thread, and the other end is provided with a negative thread, and the two adjusting rods 422 are respectively passed through the two second pressure plates 421, and the two second pressure plates 421 and the two adjusting rods 422 are parallel to each other.

[0057] Specifically, the two adjusting rods 422 are respectively threadedly connected with the second pressing plates 421 adjacent thereto, the two second pressing plates 421 are simultaneously placed in the fixture 2 and distributed at the two opposite side walls of the fixture 2, the two second pressing plates 421 and the side walls of the fixture 2 adjacent thereto are respectively provided with buffers 423, the two ends of the adjusting rod 422 are respectively rotatably connected with the side walls of the fixture 2 adjacent thereto, and the end of the adjusting rod 422 extending outside the fixture 2 is provided with a driven bevel gear 424. More specifically, a mounting seat 425 is fixed outside the side wall of the fixture 2, a driving shaft 426 is rotatably connected to the mounting seat 425, and driving bevel gears 427 are respectively provided at the two ends of the driving shaft 426, so that the driving bevel gear 427 is meshed with the driven bevel gear 424 adjacent thereto.

[0058] When in use, the active shaft 426 is rotated, and the active bevel gear 427 can rotate, thereby driving the two driven bevel gears 424 to rotate, and the adjustment rod 422 on the driven bevel gear 424 can also rotate, thereby driving the two second pressure plates 421 to move closer or farther. In the present application, two sets of pressing components 4 are provided in the clamp 2, so that the multiple sets of stacked composite structures 1 placed in the four second pressure plates 421 can be squeezed by the clamp until the outer end surface of the magnetic core material 11 is flattened, thereby forming a rectangular magnetic core material 11 with a more stable structure.

[0059] S4: Heat treatment: placing the laminated composite structure 1 in a heat treatment furnace for heat treatment.

[0060] The processing step of S4 includes the following steps: S4.1: First, evacuate the cavity of the heat treatment furnace, and then introduce inert gas into the cavity, wherein the inert gas includes nitrogen and argon. When the temperature in the heat treatment furnace is below 500°C, nitrogen is introduced; when the temperature in the heat treatment furnace is above 500°C, argon is introduced.

[0061] The prior art only introduces one inert gas during the heat treatment of the nanocrystalline magnetic core, and for cost considerations, only nitrogen is often used. However, when the temperature of nitrogen is above 500°C, nitrogen will produce nitrogen oxides, which will oxidize the magnetic core into light blue, causing serious oxidation of the magnetic core and a significant decrease in low-frequency magnetic permeability. Compared with the prior art, the present application flexibly selects to introduce nitrogen or argon according to the temperature in the heat treatment furnace, which can better protect the magnetic core material from oxidation or other chemical reactions. Moreover, the present application utilizes the characteristics that nitrogen and argon have different protective effects at different temperatures, making the protective effect more accurate and efficient, and can effectively reduce the pollution and oxide layer formation on the surface of the magnetic core, thereby improving the quality and electrical performance of the magnetic core.

[0062] S4.2: When the temperature reaches the starting temperature, place the entire fixture 2 in the cavity.

[0063] S4.3: Set at least one preset temperature node, increase the temperature gradually and sequentially, and maintain it for a period of time until the last preset temperature node is reached.

[0064] In this application, the last predetermined temperature node is set to 480°C in the heat treatment furnace and maintained for 12 hours, while adding a magnetic field to the cavity. This operation can give the atoms inside the core material enough time and energy to rearrange and adjust the structure, optimize its microstructure, improve magnetic properties and mechanical properties, help eliminate stress and defects inside the material, and improve the uniformity and consistency of the core, thereby ensuring that the core material reaches a stable crystal structure state, thereby improving its stability during use.

[0065] S4.4: Cool down to a cooling temperature node.

[0066] Specifically, when the magnetic core raw material 11 that has been solidified and shaped is taken out of the heat treatment furnace, the temperature of the nanocrystalline magnetic core is maintained above 300°C. By taking out the magnetic core at a certain high temperature, the present application can utilize the remaining heat for subsequent surface treatment or other steps requiring heat assistance, thereby improving energy efficiency and processing efficiency. In addition, it can reduce the thermal stress caused by rapid temperature changes, thereby reducing the risk of cracking or deformation of the magnetic core, and ensuring the quality and performance of the magnetic core.

[0067] When applied, by first evacuating the heat treatment furnace chamber and then introducing inert gas, the chemical reaction of the magnetic core material with oxygen or other active gases in the air during the heat treatment process can be effectively reduced to ensure the purity and performance stability of the magnetic core; by setting multiple preset temperature nodes and gradually increasing the temperature in sequence, while increasing the magnetic field at a specific temperature, this treatment method can finely control the microstructure and magnetic properties of the magnetic core, and realize the transformation from an amorphous nanocrystalline magnetic core to a nanocrystalline magnetic core. In addition, the gradual increase in temperature during the heat treatment process helps to reduce the thermal stress of the magnetic core to prevent the magnetic core from cracking or deforming during the heat treatment process. Finally, the temperature is reduced to a cooling temperature node to ensure that the magnetic core can cool slowly after the heat treatment, avoid internal stress caused by rapid cooling, and further ensure the quality and performance of the magnetic core.

[0068] S5: Dipping paint treatment: placing the laminated composite structure 1 after the heat treatment in a vacuum pressure dipping paint device for dipping paint treatment.

[0069] S6: Curing and shaping: The laminated composite structure 1 after varnish dipping is baked and cured, and then the laminated composite structure 1 is disassembled from the fixture 2, and then the cured and shaped magnetic core raw material 11, the first pressing sheet 12, the second pressing sheet 13, and the core 14 are decomposed, and the cured and shaped magnetic core raw material 11 is formed into a nanocrystalline magnetic core.

[0070] Specifically, the laminated composite structure 1 is first immersed in the hardening liquid for 1 minute. The hardening liquid can fill the tiny pores inside the material, and then filtered for 30 minutes until the hardening liquid penetrates into the microstructure of the magnetic core raw material 11, which helps to improve the density and mechanical properties of the material; in the processing step S6, the laminated composite structure 1 after paint is placed in a drying furnace for baking. The temperature in the drying furnace is maintained at 140°C for 10 hours, which can ensure that the hardening liquid is evenly solidified inside the magnetic core to form a stable structure.

[0071] S7: Surface treatment: remove the redundant insulating paint on the surface of the nanocrystalline magnetic core, and perform surface loss reduction treatment and surface protection treatment on the nanocrystalline magnetic core to obtain a finished magnetic core.

[0072] Specifically, spraying treatment is performed on 20-30 μm of the surface of the nanocrystalline magnetic core. Through spraying treatment, a uniform and dense protective layer can be formed on the surface of the nanocrystalline magnetic core, which can effectively isolate oxygen, moisture and other corrosive substances in the external environment, thereby extending the service life of the magnetic core, and controlling the spraying thickness within the range of 20-30 μm can ensure that the protective layer has sufficient thickness to provide good protection effect, which helps to reduce production costs.

[0073] In the present application, the quality of the raw material 11 is ensured by strict screening of the core material to ensure that the raw material is burr-free, dry and has a thickness within a specified range, which helps to ensure the performance and stability of the final product. The stacking and shaping method is adopted so that multiple core materials 11 can be stacked tightly and neatly together. At the same time, the end surface flattening treatment is performed to ensure the flatness and consistency of the core material 11. Affected by the material of the core material 11, the core material 11 is deformed after being subjected to pressure, so that the annular core is transformed into a rectangular core. Through heat treatment, the internal organizational structure of the core can be improved, and its mechanical and magnetic properties can be improved. The varnishing treatment can enhance the insulation performance and corrosion resistance of the core. The baking and curing makes the varnish layer more firmly attached to the surface of the core to improve the durability and reliability of the core, thereby realizing the transformation from an amorphous nanocrystalline core to a nanocrystalline core, while maintaining the shaping without restoring the deformation. Finally, by removing redundant insulating paint, surface loss reduction treatment and surface protection treatment are performed to further optimize the surface quality of the core, which helps to reduce the loss caused by friction and corrosion during use.

[0074] Compared with the prior art, through the processing steps of incoming material inspection, lamination and shaping, end face flattening, heat treatment, paint dipping, curing and shaping, and surface treatment, the magnetic core raw material 11 can be processed in batches, so that it can be transformed from an easy-to-produce ring structure into a rectangular structure, and the mechanical properties of the transformed structure are stable, and it is not easy to rebound. The finished product quality is good, and the magnetic flux path of the rectangular structure magnetic core also becomes uniform. After the above steps are processed, the processing of the amorphous nanocrystalline magnetic core can be guaranteed to be convenient, and at the same time, the magnetic flux path of the magnetic core is made uniform, the difficulty of winding is reduced, the performance of the magnetic core is enhanced, and it meets the production needs.

[0075] The above are all preferred embodiments of the present application. The embodiments are only explanations of the present application and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a square nanocrystalline magnetic core common mode inductor, characterized in that: The construction steps include: S1: Incoming material inspection: The surface of each magnetic core material (11) is free of burrs and kept dry, and the single-side thickness of the magnetic core material (11) is controlled within the specified range; S2: stacking and shaping: inserting the core (14) into the first pressing sheet (12), stacking a plurality of the magnetic core materials (11) on the first pressing sheet (12) in sequence, placing the core (14) in the middle of the magnetic core materials (11), then taking a second pressing sheet (13) and arranging it at an end away from the first pressing sheet (12), and plugging the second pressing sheet (13) and the core (14) into each other to obtain a stacked composite structure (1); S3: end surface flattening: placing the plurality of the stacked combined structures (1) in sequence in the fixture (2), spacing two adjacent stacked combined structures (1) by means of a clamping plate, and performing a flattening process on the end surfaces of the plurality of stacked combined structures (1) simultaneously by means of a material pressing assembly (4); S4: heat treatment: placing the laminated composite structure (1) in a heat treatment furnace for heat treatment; S5: varnishing treatment: placing the laminated composite structure (1) after the heat treatment in a vacuum pressure varnishing device for varnishing treatment; S6: Curing and shaping: the laminated composite structure (1) after the varnish dipping is baked and cured, then the laminated composite structure (1) is disassembled from the fixture (2), and then the cured and shaped magnetic core raw material (11), the first pressing sheet (12), the second pressing sheet (13), and the core (14) are decomposed, and the cured and shaped magnetic core raw material (11) is formed into a nanocrystalline magnetic core; S7: Surface treatment: removing redundant insulating paint on the surface of the nanocrystalline magnetic core, and performing surface loss reduction treatment and surface protection treatment on the nanocrystalline magnetic core to obtain the finished magnetic core.

2. The method for preparing a square nanocrystalline magnetic core common mode inductor according to claim 1, characterized in that: In the processing step S2, the first pressed sheet (12) and the second pressed sheet (13) have the same shape and structure, and are twice the weight of the magnetic core raw material (11).

3. The method for preparing a square nanocrystalline magnetic core common mode inductor according to claim 2, characterized in that: The core (14) comprises at least two core bodies, the core bodies are detachably connected to each other, and the core (14) presents a rectangular structure as a whole.

4. The method for preparing a square nanocrystalline magnetic core common mode inductor according to claim 3, characterized in that: The core (14) comprises a first core body (141), a second core body (142) and a third core body (143); the first core body (141) and the second core body (142) are right-angled trapezoidal structures of the same shape and size; the third core body (143) is an isosceles trapezoidal structure; the first core body (141), the second core body (142) and the third core body (143) are arranged at the same height; in the processing step S2, one waist surface of the third core body (143) abuts against the inclined surface of the first core body (141), and the other waist surface of the third core body (143) abuts against the inclined surface of the second core body (142); the three are assembled to form a rectangular structure; the outer edges of the first core body (141) and the second core body (142) are both rounded and abut against the inner wall of the magnetic core material (11).

5. The method for preparing a square nanocrystalline magnetic core common mode inductor according to claim 3, characterized in that: The processing step of S4 includes the following steps: S4.1: first evacuate the cavity of the heat treatment furnace, and then introduce inert gas into the cavity; S4.2: When the temperature reaches the starting temperature, placing the entire fixture (2) in the cavity; S4.3: setting at least one preset temperature node, gradually increasing the temperature in sequence, and maintaining the temperature for a period of time until the last preset temperature node is reached; at the same time, adding a magnetic field to the cavity; S4.4: Cool down to a cooling temperature node.

6. The method for preparing a square nanocrystalline magnetic core common mode inductor according to claim 5, characterized in that: The inert gas includes nitrogen and argon. In the processing step S4.1, when the temperature in the heat treatment furnace is below 500° C., nitrogen is introduced; when the temperature in the heat treatment furnace is above 500° C., argon is introduced.

7. A method for preparing a square nanocrystalline magnetic core common mode inductor according to claim 5 or 6, characterized in that: In the processing step S4.3, the temperature in the heat treatment furnace is maintained at 480° C. for 12 hours.

8. A method for preparing a square nanocrystalline magnetic core common mode inductor according to any one of claims 5 or 6, characterized in that: In the processing step S4.4, when the magnetic core raw material (11) is taken out of the heat treatment furnace after solidification, the temperature of the nanocrystalline magnetic core is maintained above 300°C.

9. A method for preparing a square nanocrystalline magnetic core common mode inductor according to any one of claims 1 to 5, characterized in that: In the processing step S5, the laminated composite structure (1) is first immersed in a hardening liquid for 1 minute, and then drained for 30 minutes until the hardening liquid penetrates into the microstructure of the magnetic core raw material (11); in the processing step S6, the laminated composite structure (1) after varnishing is placed in a drying furnace for baking, and the temperature in the drying furnace is maintained at 140° C. for 10 hours.

10. A method for preparing a square nanocrystalline magnetic core common mode inductor according to any one of claims 1 to 5, characterized in that: In the processing step S7, 20-30% of the surface of the nanocrystalline magnetic core is sprayed.

Citation Information

Patent Citations

  • Paint impregnating fixture of transformers

    CN105895350A

  • Nanocrystalline magnetic core and preparation method thereof

    CN110931238A

  • Preparation method of laminated amorphous and nanocrystalline iron core

    CN114977685A

  • C-type iron core solidifying and molding device

    CN202905455U

  • Rapid shaping and annealing tool clamp for amorphous or nanocrystalline magnetic core

    CN218507858U